Thickness                              10mm (WPS qual. 10-20mm)

Mat                                        Plate - SA516 Gr60 & SA516 Gr70 (this will qualify bot P1G1 and P1G2 mats right?)

you can not do this in your case as Impact test is required and G no is SEV.


Preheat                                  38°C Min(client spec)

Interpass Temp                       250°C Max

PWHT                                   620°C (120min, 100°C/hr)

PWHT should be determined as per cinstruction code.
If it is Div 1 follow UCS table for P no 1 material

Pos                                       3G (NON Essential Variable.)

Type                                      GTAW + SMAW

 

Tests:

2              Tensile Test

2              Face Bend Test

2              Root Bend Test

4              Side Bend Test (Do we need this?)

5?           Toughness Test (Charpy V-Noch at -46 C is enough?) at MDMT

Other DT should be as per QW-451.1


Hardness

Radiography


And the other thing is how big test coupon should I weld to get these tests.

On Fri, Feb 1, 2013 at 8:00 AM, Tarık Tuna <tariktuna@gmail.com> wrote:
Dear Experts,

Our company is going to make a new PQR and WPS but since I am new at ASME sec IX and B31.3, I would like to verify my tests before doing them.

So PQR specs are;

Thickness                              10mm (WPS qual. 10-15mm)

Mat                                        Plate - SA516 Gr60 & SA516 Gr70 (this will qualify bot P1G1 and P1G2 mats right?)

Preheat                                  38°C Min(client spec)

Interpass Temp                       250°C Max

PWHT                                   620°C (120min, 100°C/hr)

Pos                                       3G

Type                                      GTAW + SMAW

 

Tests:

2              Tensile Test

2              Face Bend Test

2              Root Bend Test

4              Side Bend Test (Do we need this?)

5?           Toughness Test (Charpy V-Noch at -46 C is enough?)

Hardness

Radiography


And the other thing is how big test coupon should I weld to get these tests.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 



--
Thanks & Regards
Biplab Pal
Welding Inspector
E-mail:   biplab.mech@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

[MW:34866] Presentation for WPS ,PQR AND WPQ as per ASME Sec IX in power point

Dear Experts.        If anyone having presentation of WPS,PQR and WPQ  as per ASME  SEC.IX  in power point then please share . Regards Sanja...