Thursday, January 3, 2013

Re: [MW:16413] RE: 16411] HardnessP-91 Material

 
This is not addressed in code. But typically
Base metal - 210-265 HB
Weld metal & HAZ - 210 0 300 HB
Good results can be achived if you can maintain max difference of 30HB between all three i.e. BM, WM & HAZ.

Raghava
On Thu, Jan 3, 2013 at 7:21 AM, Ryan Carbonara <rcarbonara@valv.com> wrote:

Client call typically. You wont find it in B31.1

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Anthony Rudder
Sent: Wednesday, January 02, 2013 11:37 AM
To: materials-welding@googlegroups.com
Subject: [MW:16411] HardnessP-91 Material

 

Sir,

What's the Max hardness for weld metal and HAZ for P-91 Material per B31.1

 

 

 

 

Thank You,

 

Tony

QA.Manager.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:34866] Presentation for WPS ,PQR AND WPQ as per ASME Sec IX in power point

Dear Experts.        If anyone having presentation of WPS,PQR and WPQ  as per ASME  SEC.IX  in power point then please share . Regards Sanja...