Dear Ankit,
 
In addition to the earlier mail i want to add
 

323.3.5 Acceptance Criteria

(c) Weld Impact Test Requirements.

Where two base metals having different required impact energy values are joined by welding, the impact test energy requirements shall conform to the requirements of the base material having a specified minimum tensile strength most closely matching the specified minimum tensile strength of the weld metal.

Nothing says about Lateral Expansion.

 



On Thu, Nov 1, 2012 at 9:58 AM, Ankit PAtel <ankit.patel@orientalindia.net> wrote:

Dear Experts,

 

We have performed a PQR for 25 thk  plate , P1(SA 516 GR-70 ) To P8(SA 240 TP-316L). These PQR has been stress relieved at 620° C & impact tested at -20°C.

The testing laboratory has noted down only the joule values for the impact test, but they have not noted the Lateral Expansion Values P-8 Material.

The Avg. Joules Values observed are as follows:

Weld-72.67 J

HAZ(GR-70)-35.33J

HAZ(GR-316L)-158 J

PARENT(GR-70)-51.33J

PARENT(GR-316L)-298 J

 

Now our TPI says that for GR-316L Lateral Expansion Values is must for acceptance of the PQR.

Is it so?

Or based on these joules values these PQR can be accepted & used for weld having requirement of impact  test at -20°c

 

 

Thanks & Regards

Ankit Patel
Engineer Quality

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 



--
Thanks & Regards
Biplab Pal
Welding Inspector
E-mail:   biplab.mech@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

Re: [MW:34832] Inquiry about Single Bevel with Back Grinding

Dear Uday, As per your question that one is called with backing only,Simple both side you are welding it is backing with strip or without st...