Re: [MW:15831] requirment of Lateral expansion for P1 TO P8 PQR as ASME Sec IX

Lateral Expansion may be 0.38 mm

On Thu, Nov 1, 2012 at 12:28 PM, Ankit PAtel <ankit.patel@orientalindia.net> wrote:

Dear Experts,

 

We have performed a PQR for 25 thk  plate , P1(SA 516 GR-70 ) To P8(SA 240 TP-316L). These PQR has been stress relieved at 620° C & impact tested at -20°C.

The testing laboratory has noted down only the joule values for the impact test, but they have not noted the Lateral Expansion Values P-8 Material.

The Avg. Joules Values observed are as follows:

Weld-72.67 J

HAZ(GR-70)-35.33J

HAZ(GR-316L)-158 J

PARENT(GR-70)-51.33J

PARENT(GR-316L)-298 J

 

Now our TPI says that for GR-316L Lateral Expansion Values is must for acceptance of the PQR.

Is it so?

Or based on these joules values these PQR can be accepted & used for weld having requirement of impact  test at -20°c

 

 

Thanks & Regards

Ankit Patel
Engineer Quality

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:34916] Applicability of Impact requirement as per ASME B31.3

Dear All, Design code – ASME B31.3, Welding Code- ASME BPVC SEC IX Material  to be used used during Fabrication - SA 333Gr6 (P No.1 G...