Dear Experts,

 

We have performed a PQR for 25 thk  plate , P1(SA 516 GR-70 ) To P8(SA 240 TP-316L). These PQR has been stress relieved at 620° C & impact tested at -20°C.

The testing laboratory has noted down only the joule values for the impact test, but they have not noted the Lateral Expansion Values P-8 Material.

The Avg. Joules Values observed are as follows:

Weld-72.67 J

HAZ(GR-70)-35.33J

HAZ(GR-316L)-158 J

PARENT(GR-70)-51.33J

PARENT(GR-316L)-298 J

 

Now our TPI says that for GR-316L Lateral Expansion Values is must for acceptance of the PQR.

Is it so?

Or based on these joules values these PQR can be accepted & used for weld having requirement of impact  test at -20°c

 

 

Thanks & Regards

Ankit Patel
Engineer Quality

 

 

No comments:

Re: [MW:34832] Inquiry about Single Bevel with Back Grinding

Dear Uday, As per your question that one is called with backing only,Simple both side you are welding it is backing with strip or without st...