RE: [MW:15257] maximum and minimum size of Dish end end SPIN hole plate.


Dear sutar,
 
CC: Sanjay Yadav - Pl read specification not specified minimum size..

 

Spin-holes not greater in diameter than 238 in. (60 mm) may be closed with a full-penetration weld using either a welded plug or weld metal. The weld and pug shall be no thinner than the head material adjacent to the spin-hole.

 

The finished weld shall be examined7 and shall meet the acceptance requirements of Appendix 6 or Appendix 8 of this Division. Radiographic examination, if required by UW-11(a), and additional inspections, if required by the material specification, shall be performed. This weld is a butt weld, but it is not categorized. It shall not be considered in establishing the joint efficiency of any part of the head or of the head-to-shell weld.





Thank & Best Regards,

 

M Veera SAMY- Bureau Veritas.

Coimbatore

 

 


 

Date: Sun, 9 Sep 2012 22:20:11 +0530
Subject: Re: [MW:15254] maximum and minimum size of Dish end end SPIN hole plate.
From: ssy070707@gmail.com
To: materials-welding@googlegroups.com

dear sutar,

there is no maximum dia limit for spin holes in dished ends as per code. generally it ranges from 25 mm to 40 mm.
if there is no nozzle at that location than patch shall be welded and 100% radiographed which is code requirement.

Regards
Sanjay Yadav

On Thu, Sep 6, 2012 at 9:16 AM, hemant <hsuthar@chemithon.co.in> wrote:

Dear Sir,

What is the minimum  & Maximum size of spin hole plate as per code reference. Pls reply me.

 

HEMANT SUTHAR

QA/QC

CEPL-SILVASSA

9712973092

 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

Re: [MW:34913] Filler wire

E71T-1C  is Charpy Impact tested at -20degC E71T-1CJ is Charpy impact tested at -40degC. AWS Classification for FCAW is only a supplementary...