You can use E 7016 -A1 or E 7018-A1 for P22 to CS.
Alternatively, E 8016 -B2 or E 8018-B2 is also recommended.
sridhar.
From: hany karica <hany_karica@yahoo.com>
To: materials-welding@googlegroups.com
Sent: Sunday, 8 July 2012 6:38 PM
Subject: Re: [MW:14807] Filler wire for pipe alloy steel (P22) to cs (P1)
dear experience
E9018 B3 used for welding p22 to A106
From: Bijay <bkchoudhury80@yahoo.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Sunday, July 8, 2012 3:56 AM
Subject: [MW:14805] Filler wire for pipe alloy steel (P22) to cs (P1)
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
E9018 B3 used for welding p22 to A106
From: Bijay <bkchoudhury80@yahoo.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Sunday, July 8, 2012 3:56 AM
Subject: [MW:14805] Filler wire for pipe alloy steel (P22) to cs (P1)
Dear Experts,
Kindly suggest me which filler wire best suitable for dissimilar metal pipe joints P22 to cs SA106 Gr B
Awaiting for your valuable answer
With Regards
Bijay Kumar Choudhury
Mob +91 94084 43554
Mob +91 89806 30973
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
No comments:
Post a Comment