Re: [MW:14571] filler used to weld cast iron pipe to SS pipe

ERNiCr-3 for root pass and 2nd pass,
then ER309L for others pass and cover pass.
 
--
George Xue (Xue Guoliang)
Suzhou CXGL Mechanical Engineering Co., Ltd.
Purchasing and Engineering Manager
Tel: +86-512-68639769 Fax: +86-512-68639492
Skype: xuegl2001
 

2012/6/15 Saravanan Sornam <saravanshyla@gmail.com>
Hi Manoj,
 
Refer ASME - II C, SFA 5.15 Appendix A7.2.3
 
ENiFe-CI (Nickel-Iron) Classification. This
electrode may be used for making repair welds on, as well
as for joining, work pieces of various types of cast iron,
including nodular iron, and for welding them to steel and some nonferrous base metals. Castings containing phosphorus
levels higher than normal (approximately 0.20%
phosphorus) are more readily welded using these electrodes
than with an electrode of the ENi-CI classification. Experience
has shown that satisfactory welds can be made on
thick and highly restrained weldments, and on highstrength
and engineering grades of cast iron.
 
It's better consult the technical person from ESAB or other consumable brand persons for the exact AWS class either for GTAW or SMAW.
 
Hope this one helps...
 
Cheers,
Saravanan,
Korea
On Thu, Jun 14, 2012 at 7:22 PM, Manoj G <manojj.24g@gmail.com> wrote:
Dear all,

Please suggest me the filler to be used to join cast iron pipe with Stainless steel 304 pipe of  5 mm thickness.


Manoj.G

QA/QC

Petron Engineering Construction Ltd.
APML Site Tiroda


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Blog Archive