RE: [MW:14201] Welding C45 (1045)

Hi,

 

You can do post cooling with wrapping a glass wool at weld joint- immediate after welding completion. This will also help to resist crack in this higher carbon steel.

 

Best Regards,  

 

Vimal Mistry

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of prem nautiyal
Sent: 07 May 2012 15:40
To: materials-welding@googlegroups.com
Subject: Re: [MW:14199] Welding C45 (1045)

 

Hi

 

Increase the preheat to 150 degrees Celcius min. Interpass temp 250 degrees celcius max.

Use SMAW E7018-1 electrode.

 

I have successfully welded C45 material with E7018-1.

 

Regards

 

Prem Nautiyal

 

From: LeONarD P <metpick@gmail.com>
To: Materials & Welding <materials-welding@googlegroups.com>
Sent: Saturday, May 5, 2012 10:56 AM
Subject: [MW:14187] Welding C45 (1045)


Dear All expert

        Welding C45 (1045) steel (Pivot Boss) to S275JR (main
structure)

1045 Pivot Boss is casting part.
S275JR is steel plate

For a project I need to weld a C45 (1045 steel, 0.45% carbon Thick 100
mm) on a S275JR steel ( Thichness 30 mm.)

Joint design & condition weld:  T-butt joint, double bevel, CJP. Bevel
at S275JR steel.
                                                  preheat 110 C
minimum,. interpass temp 220 C max.
                                                  by FCAW process.
A5.20 / E71T-1C


      After weld, the problem is crack appear along on surface casting
part (1045 steel)

How to solve this problem.

Thank you very much.
leonardd..

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


------Disclaimer-------
This email and any files transmitted with it are confidential and may be privileged or otherwise protected from disclosure and are intended solely for the use of the entity / individual to whom they are addressed. If you have received this email in error or If you are not the intended recipient, please notify the sender immediately by way of telephone or email and delete this message and any files transmitted from your system. Please note that any views presented in the email are solely those of the author and do not necessarily represent those of the organization. While all care has been taken to avoid viruses the recipient is advised to check this email and attachments for presence of viruses. The organization accepts no liability on this account.
------Disclaimer-------

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...