Hi Eswaran,
 
These two are the important among the applicable clauses for local PWHT. As stated here and as required a as a part of the quality documentations a PWHT procedure is required.It should include as a minimum requirement the following:-
  1. mode of heating   
  2. ramp rates(both heating and cooling)
  3. recommended PWHT time and temperature, Item 1,2,3 should be as per the design code
  4. no of  thermocouples required, location, width of the heating band etc(one may follow AWS D-10.10) as a default standard.
If the client has a written procedure , one should follow that. In case of  a  technical conflict , AWS D-10.10 may also  be referred.
 
Thanks.
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist & Consultant

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

6.3.3.4 Post-weld heat treatment — Local heating Local post-weld heat treatment shall consist of heating a circumferential band around the weld at a temperature within the range specified in the qualified WPS. The minimum width of the controlled band at each side of the weld on the face of the greatest weld width shall be the thickness of the weld or 50 mm (2 in) from the weld edge, whichever is less. Heating by direct flame impingement on the material shall not be permitted.

6.3.2.6 Post-weld heat treatment Post-weld heat treatment shall be in accordance with the applicable qualified WPS. Welds may be locally post-weld heat-treated. The manufacturer shall specify procedures for the use of local postweld heat treatment.



From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of K.Babu
Sent: Friday, March 02, 2012 9:07 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:13808] Post Weld heat treatment & No of thermocouples regarding

Hi
 
We need to refer client spec for this job.
 
VG, Cameron got their own spec for PWHT.
 


 
On Fri, Mar 2, 2012 at 2:28 PM, Eswaran samikannu <eswaranaws@yahoo.co.in> wrote:
Good day to all,
 
We are one of the authorised repairing & Manufacturer  of OEM Cameron, VG & Shaffer BOP and riser pipes , I want to know thermocouples location / No of thermocouples vs Pipe size according to API 6A /API 16A for localaised stress relief (PWHT), Any one have the standards let me know or inform where i can get the information.
 
Thanks
S.Eswaran 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Thanks & regards,

K.Babu

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...