In my experience, there is no single “best” portable hardness tester.  Below are several I have worked with and their +’s from my experience:

 

EquoTip         (Leeb type)

+  small, light weight, user friendly, different indenters depending on application

-  needs correction for direction, operator sensitive, needs surface prep for repeatability,  will read significantly low if there is insufficient mass in direction of test

 

Krautkramer MIC10    (ultrasonic, resonant frequency type)

+  small, light weight, user friendly, indent virtually un-noticeable

-  very sensitive to surface prep adequate grinding required for repeatability, may not be useable in some close quarters applications, operator sensitive

 

RockMate

+  simulates standard Rockwell test, portable, user friendly, less sensitive to surface prep than EquoTip or MDC10, not particularly sensitive to operator

-  bulkier than EquoTip or MIC10, requires much larger foot print than EquoTip or MIC10, not for tight quarter use

 

The non-digital, brute force method, i.e. TeleBrineller, is still a valid method that you might want to consider. 

 

Myself, I would avoid the EquoTip (Leeb – falling ball) type.  I have too much experience with the mass effect to trust a value by this method unless the part is truly massive,  the indent orientation can put at least 6 inches (150mm) of material beneath the indenter, or the part is small enough with a flat enough area to be effectively “coupled” to a massive item.   Look at the size of calibration block that is required for  the Equotip – that thickness is required to obtain an accurate, repeatable values and is what one needs to obtain correct hardness values in the field.  EPRI and NUMARC in the 1980’s did quite a bit of testing with the EquoTip and found it too read consistently and significantly low in almost all cases. 

 

The non-digital, brute force method, i.e. TeleBrineller, is still a valid method that you might want to consider. 

 

 

Good luck.

 

John A. Henning

Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pawan
Sent: Friday, March 16, 2012 7:20 AM
To: materials-welding@googlegroups.com
Subject: [MW:13897] best portable hardness tester-digital

 

Hi,

 

Pl. suggest best digital portable hardness tester (HRC) to check the weld metal hardness on 3layers pad.

 

T&R

Pawan tiwari

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...