Dear Mr.Pradip,


Is anything wrong in accepting more diluted weld deposition with the consideration of application ?  

For example if our weld metal chemistry is meeting the requirement of Inconel 825 (weld overlay with Inconel 625) which satisfy the application condition without any failure.

Is there any test to confirm this ?


Rinshad

On Wed, Feb 15, 2012 at 7:23 AM, pgoswami <pgoswami@quickclic.net> wrote:
Hi Budi,
 
The weld deposit should meet C.A  requirements of  AWS/ASME SFA 5.14(see below). If I could re-collect from the past experiences, meeting C.A in single pass ESSC could be a problem(see the attachment).Fe dilution is always a problem in the first pass.It would be a good point to discuss the issue with the consumable supplier prior hand and resort to multipasses, if there're severe restrictions on Fe dilution in 625 overlay.
 
See the link for the soudometal product catalogue for SAWSC and ESSSC.The attachment is a page extracted from this document.
 
What is the design code? By any chance does the C.A of the deposit has to conform to API Spec, 5LD??
 
Appreciate your feedback.
 
Thanks.
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist & Consultant

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 
 
 

Nb

(Cb)

Other

AWS Classification

m

UNS Number

C

Mn

Fe

P

S

Si

Cu

Ni

d

Co

Al

Ti

Cr

plus

Ta

Mo

V

W

Elements,

Total

 

 
 
 


On Tue, Feb 14, 2012 at 7:10 PM, <budi.witjaksono@profab-group.com> wrote:
Dear Colleague,
We do overlay inconel 625 with single layer strip cladding electroslag welding however the chemical contents on weld deposit taken from 3 mm from fusion line does not comply exactly to the chemical composition of Inconel 625.
I have checked the weld deposit chemical composition data from the strip cladding supplier also does not exactly comply to Inconel 625.
Is anyone can tell me what is the chemical composition acceptance criteria for Inconel 625?
Is it correct the weld deposit chemical contents for inconel 625 overlay should conform to ASTM B424 UNS N08825 instead of Inconel 625? If yes, is there any reference standard I can refer to?
Regards,

Budi Witjaksono

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...