Skip to main content

Re: [MW:13620] NORMALIZING OF DIHED HEAD AFTER HOT FORMING

dear,
normalising cannot be avoided even if dish is hot formed in normalising range.
vanchi
On Mon, Feb 6, 2012 at 12:28 PM, asad azmi <azmiasadayub@gmail.com> wrote:
Dear All,
 
Greetings.
 
A Vessel has to be fabricated as per ASME SEC VIII DIV 1.  Vessel requires SPWHT as per Client requirment.
 
 A Dished head of material SA 387 GR 12 CL2, Normalized and Tempered - 80  mm Thickness, has been HOT Formed at temperature 920 deg. Celsius
 
As per Hot Forming Procedure after reaching soaking temperature of 920 deg celsius and holding for 1 hour,  Hot forming operation was performed outside the furnace and immediately after hot forming dished head was put back in the furnace and  temperature was again increased upto 920 dec celsisus before transferring dished head in Shop Floor for  cooling.
 
As per ARAMCO Standard Noramilizing and tempering  shall be perforemd as seprate operation after Hot forming as per below clause.
 
13.2.14.1 Heat-treatment, as a separate operation, shall be performed after a forming operation (hot or cold) for any of the conditions listed below. The heat treatment shall be annealing, normalizing, normalizing and tempering, or quench and tempering, as required.
 
Please be informed that as per hot forming procedure Noramalizing after forming has to be performed at 920 Deg Celsius.
 
Contractor has not performed Normalizing sepratley after Hot forming.  as per reports test coupon has also undergone only ONE Normalizing Cycle.
 
Please advise whther Normalizing can be avoided as the hot forming was done at Normalizing temperature. 
 
As per ARAMCO requirement Heat treatment cycle  for Dished head & Test coupon should be  Hot forming  + Normalizing + tempering + SPWHT.
 
Please suggest.
 
Thanks in advance.
 
Regards
 
Asad Azmi

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...