Re: [MW:13412] Hydro testing failure

The answer given by Morin Darcy seems to be valid reason, and truly seems that its only a single pass weld which is not acceptable.

On Tue, Jan 3, 2012 at 6:02 PM, Morin, Darcy (Bantrel Management Services) <MorinD@bantrelmanagementservices.com> wrote:
If there is a through-thickness pinhole, and your welding process is GTAW, the pinhole is most likely not caused by a lack of shielding gas or contamination.  This type of pinhole on a groove weld is caused by the arc is being removed suddenly from the molten pool, resulting in a heat shrinkage pinhole. 
 
This can be corrected by:
 
1.  The welder gradually reducing the amperage as he terminates the arc (throttling down with his thumb throttle on the GTAW torch handle).
 
2.  Travelling forward with the arc after he ties in to close the root bringing the molten puddle on top of solid metal.
 
When this defect occurs, with hydrotest failure, it usually indicates that the weld was performed with only one pass.  Some Specifications require that pressure retaining welds be performed by no fewer than 2 passes. Investigate the welder's work practice.
 
Darcy Morin
 
Bantrel Management Services
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Dick Overkleeft
Sent: December 27, 2011 1:10 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:13339] Hydro testing failure

Dear Mr. Shankar,
 
The porosity can be caused, by the following causes;
1) dirty or not clean piping or filler rod
2) unsufficient gasprotection  from the torch
3) unsufficient backing gas
other causes may be excluded.
 
best regards,
 
Dick Overkleeft

2011/12/27 Dinesh Ravi Shankar <dinesh_ravi2001@yahoo.com>

Thank you jesti.
 
I already verified PMI reports,but it is 2" line so we cannot check pmi under root pass.& may be after 2/3 days RT taken after welding.
 
yes thru PT one round indication found on capping...after some grinding also its going like pin hole. thats y i m asking that in GTAW process,how pin holes will occur..? we have to avoid such a things during welding. 
 
Thank you & Best Regards,

S. Dinesh Ravi Shankar.
Mechanical Inspector,
Saudi Aramco Project Inspection Division (SAPID),
Manifa Core Hydrocarbon Facilities Project.
Kingdom of Saudi Arabia.,
Mobile : +966 562944695,

Tel      : +966 3 379 2018.
 
  
 

From: jesti fer <jesti_fer@yahoo.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Tuesday, December 27, 2011 8:05 AM
Subject: Re: [MW:13320] Hydro testing failure

Dear Mr. Shankar,
Is it possible to check the PMI in root weld, (the welder may use CS filler wire for root pass) and what is the time duration between completion welding and RT. You are getting any indication in PT?
 
Best regards
K>M>H

From: Muhammad Ashraf <mohdashrafr@gmail.com>
To: materials-welding@googlegroups.com
Sent: Monday, December 26, 2011 1:35 PM
Subject: Re: [MW:13313] Hydro testing failure

IT MIGHT BE DUE TO (Microbiologically Influenced Corrosion) MIC. LET ME KNOW IF YOU HAVE CARRIED OUT FLUSHING AFTER HYDROTEST AS RESIDUAL WATER, AT LOW POINTS IN THE 300 SERIES PIPING, LEADS TO SUCH FAILURES.
 
 
RANA
 
 
On Mon, Dec 26, 2011 at 8:57 AM, Dinesh Ravi Shankar <dinesh_ravi2001@yahoo.com> wrote:

 Thank you Mr.Karanth for excellent information.
 
Anyway as per catagory we cannot cover 100% RT,but we have to avoid such a things during welding.In GTAW process,how pin holes will occur..?
 
Dinesh.
   

From: shankar narayan karanth <karanthequipments@gmail.com>
To: materials-welding@googlegroups.com
Sent: Sunday, December 25, 2011 4:57 PM
Subject: Re: [MW:13308] Hydro testing failure

Dear Shankar,

  It looks that there are pin holes  which you might have considered them to be rounded indication with in the limits of acceptance while Radiography interpretation.When optical density of rounded indication is quite high, you have to suspect them to be pin holes and had you carried PT on them it is quite likely that you have detected the defects.It is quite likely that very small rounded indications may not get picked up while carrying out MT. Hope this has answered your query.

P.S.Karanth
98251 29987

On Sun, Dec 25, 2011 at 5:41 PM, Dick Overkleeft <dick.overkleeft@gmail.com> wrote:
Dear Mr. Shankar,
 
Could you please sent some more information?
Can you inform us what kind of stainless steel you applied.
What welding process you used, and which filler material.
Is it plate or tube welding.
What kind of water ( is there any chlorid in the water) did you use for hydrotesting and did you air test before hydrotesting.
What kind of defects did you see on the X-ray?
 
After this we might be able to give an answer on your question.
 
bets regards,
 
Dick Overkleeft EWE
Bureau Veritas

2011/12/24 Dinesh Ravi Shankar <dinesh_ravi2001@yahoo.com>
 
Dear friends,
 
During hydro testing of stainless steel, recently 2 tests leak occurred at welded joint area. I verified RT films, PMI reports...etc.Just I want to find root cause.
 
Please advise me that what proactive surveillance need to take of further hydro test failure & how it is happening..?
 
 
 
Thank you & Best Regards,

S. Dinesh Ravi Shankar.
Mechanical Inspector,
Saudi Aramco Project Inspection Division (SAPID),
Manifa Core Hydrocarbon Facilities Project.
Kingdom of Saudi Arabia.,
Mobile : +966 568059765,
Tel      : +966 3 379 2018.
 
  
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

This e-mail and any attachments may contain confidential and
privileged information. If you are not the intended recipient,
please notify the sender immediately by return e-mail, delete
this e-mail and destroy any copies.

Any dissemination or use of this information by a person other
than the intended recipient is unauthorized and may be illegal.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...