RE: [MW:13379] REGARDING Impact test of VESSEL PRODUCTION TEST COUPON

Hi

 

//I
have tested a stress relieved PTC Impact test on weld & HAZ AT -47
DEG.//

 

Hope you have used Full size specimen. (10x10mm). But the material specification is missing. If it is SA 516 Gr 70, you need 20J average. In these assumed conditions you test is acceptable. BUT…

 

// PTC has failed again I have  done  reheat treatment & Retest with
same cycle of the job.//

 

So, you have done retreatment. Is it done on the same PTC or with another PTC?.

 

If reheat done on the same PTC which failed earlier, then the PTC might have received two heat treatment cycles, which is not simulating to your vessel heat treatment conditions. This is not acceptable. [refer UG-84(h)(4) & QW 407.2]. Check whether your WPS covers the T &T range.

 

If reheat treatment done on another PTC, then the test is OK.

BR

M.Vijayan

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Karthik
Sent: Wednesday, December 28, 2011 10:28 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:13348] REGARDING Impact test of VESSEL PRODUCTION TEST COUPON

 

Hi,

As per ASME Sec.VIII,Div.1-UG84, 

The minimum impact energy for one specimen shall not be less than 2⁄3 of the average energy required for three specimens. The average impact

energy value of the three specimens may be rounded to the nearest J.

 

 

Thanks & Regards,

 

(Karthik)

 

Karthikeyan.S

QA/QC Manager

Getabec Energy Co.,Ltd.

379,Moo6,Soi8,Nikhomphatana,

Rayong-21180,

Thailand.

Phone: 0066 38 897035-8 (Off)

Fax: 0066 38 897034

Hand Phone: 0066 892512282

 


From: Harish Kannepalli <harishkannepalli@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wednesday, December 28, 2011 12:08 AM
Subject: Re: [MW:13334] REGARDING Impact test of VESSEL PRODUCTION TEST COUPON

Dear Vivek,

                70% of required average is ok, ur values r ok to pass the PTC.

2011/12/27 Vivek Pandey <vivek.pande06@gmail.com>

Respected All,


I want your suggestion about Impact test of vessel production test, I
have tested a stress relieved PTC Impact test on weld & HAZ AT -47
DEG. PTC has failed again I have  done  reheat treatment & Retest with
same cycle of the job. PTC has failed in one indivzual value by 1
joule.Value is like this way 28, 19, 34.


Is there any acceptance criteria as per ASME SECTION VIII DIV 1. other
wise all weld of category A B C D to be gauged & reweld.

Kindly solve my query as soon as possible



Regards
VIVEK PANDEY

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



 

--

regards,

Harish.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



This communication and any files transmitted with it are confidential and may also be privileged. It is for the exclusive use of the intended recipient(s). If you are not the intended recipient or the person responsible for delivering it to the intended recipient(s), please note that any form of distribution, copying or use of this communication or information contained in it is strictly prohibited and may be unlawful. If you have received this communication in error please return it to the sender, and delete the material from any computer. We reserve the right to monitor email communications through normal internal and external networks. We believe but not warrant that the email and the attachments are virus free. The statement and opinions expressed in this communication are those of the writer and do not necessarily represent those of Madina Group, whose registered office address is

P.O. Box 20459, Doha, Qatar.
Tel. +974 44600818
Fax. +974 44603143

No comments:

[MW:34820] RE: 34813] Clarification in Rate of heating and cooling.

Hello,   Please see the response below.   Regards.   P. Goswami, P. Eng, IWE.   From: materials-welding@googlegroups.com <materials-weld...