Skip to main content

Re: [MW:13225] Impact test fail with A333 Gr6

Your base metal thickness is 34 mm and your deposited metal thickness is 5 mm?
This looks strange?
What is your construction code?
Usually with 35 mm thickness you need PWHT
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager


  From: solomon [soiy7777777@gmail.com]
  Sent: 16/12/2011 23:46 PST
  To: materials-welding@googlegroups.com
  Subject: [MW:13222] Impact test fail with A333 Gr6


Dear everyone
I do PQR with following data
1. pipe SA 333 Gr 6 (12" SCH. 160) and Flange SA 350 LF2
2. Joint design is single V
3. Process GTAW+SAW
4. Preheat 80C Min. with burner torch
5. With out backing gas for root pass
6. Use ER 80-S-Ni1 (BOHLER) two layer with total deposited about 5mm and 

The result of tensile, bend, marcro look very good.
Before impact test I already RT, UT, and MT to confirm that no defect
The impact test (joules) done at -46C, on the location as follow and the result as shown
FL,Root(Flange)            112,86,89
FL+2,Root(Flange)         26,61,107
FL,Root(Pipe)                25,130,12  
FL+2,Root(pipe)             24,14,19
FL,Middle(flange)            131,108,132
FL+2,Middle(flange)         194,154,200
FL,Middle(pipe)              38,56,125
FL+2,Middle(pipe)           80,124,112
WM,Root                        42,80,79
WM,Middle                     24,106,92
The acceptance criteria is average 20 and Min. 16
From the result above I have to retest again with
FL,Root(pipe)                 37,19,20
FL+2,Root(pipe)             14,12,25

So I need some help from you guides to analyze the cause of this result. In my opinion I think it may come from one of below reason
1. the preheat temperature too low due to the thickness of base mat about 34 mm so the heat dissipate very quick for GTAW. 
2. skill of welder may be not familiar with this filler (add Ni)  so the fusion to base material not deep enough even the NDE result not shown any defect
Due to I don have remaining mat. enough to do it many time I need some advice from yours
Thanks you in advance for your kind support
Bye

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...