ASTM A193 or ASTM A320 Gr. B8 or B8M cl.2 are can be used within temp. range of -196 to +300 Deg C, could you please elaborate why A320 B8M class-1can not be used for 1500#, Material selection does not depend on pressure class, for higher classes thickness would increase.
Please correct me if i am wrong.
Regards
Manpreet Singh
From: "Vinod Kataria" <vinod.kataria@blissanand.com>
Sent: Fri, 09 Dec 2011 15:10:29
To: <materials-welding@googlegroups.com>
Subject: [MW:13166] Fasteners for Nace MR0175
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
From: "Vinod Kataria" <vinod.kataria@blissanand.com>
Sent: Fri, 09 Dec 2011 15:10:29
To: <materials-welding@googlegroups.com>
Subject: [MW:13166] Fasteners for Nace MR0175
Dear All,
Please note for one of our ongoing project we have offered fasteners for our Level Gauge as ASTM A-320 Gr B8M cl-ass 2 which is suitable for low temperature and High Pressure Rating but our customer asking these fasteners conforming to NACE MR0175 also for this application ASTM A-320 Gr B8M cl-ass 1 is suitable but they cannot be used for high pressure rating i.e. 1500# so request suitable fasteners which will meet following service requirement:-
1. NACE MR0175 (Hardness Should be below 22 HRC).
2. Service Temperature -100 degree C.
3. Pressure Rating 100 bar.
Thanks in advance for your kind help.
Regards
Vinod Kataria
+91-9560199004
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
| Follow Rediff Deal ho jaye! to get exciting offers in your city everyday. |
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments