Skip to main content

Re: [MW:13150] Dissimilar welding SS 316 to A335GrP5

It would be better to butter the P5 portion say 5 mm with ENiCrMo3, perform PWHT and weld it with 316SS .
 
Thanks & Reagrds
 
J.Gerald Jayakumar
00968-93281596
From: "george.dilintas@gr.bureauveritas.com" <george.dilintas@gr.bureauveritas.com>
To: materials-welding <materials-welding@googlegroups.com>
Sent: Tuesday, December 6, 2011 12:46 PM
Subject: Re: [MW:13149] Dissimilar welding SS 316 to A335GrP5

I would not suggest to direct them directly. What are your thicknesses?
Best regards
Dr Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
HBS Regional Technical Manager
  From: "Ashok Raman B Kutty \(MNT/PPTSB\)" [ashokraman_kutty@petronas.com.my]
  Sent: 06/12/2011 09:27 ZE8
  To: <materials-welding@googlegroups.com>
  Subject: [MW:13145] Dissimilar welding SS 316 to A335GrP5

We need to weld a SS 316 Return bend to 5 Chrome, 0.5 Mo alloy steel furnace tube. The electrode proposed is ENiCrMo3. The return bends are in a header box adjacent to the radiant section (horizontal tube furnace – crude distillation unit).
 
Is PWHT required to be done after welding?
 
Thanks
 
Ashok
DISCLAIMER : This e-mail and any files transmitted with it ("Message") is intended only for the use of the recipient(s) named above and may contain confidential information. You are hereby notified that the taking of any action in reliance upon, or any review, retransmission, dissemination, distribution, printing or copying of this Message or any part thereof by anyone other than the intended recipient(s) is strictly prohibited. If you have received this Message in error, you should delete this Message immediately and advise the sender by return e-mail. Opinions, conclusions and other information in this Message that do not relate to the official business of PETRONAS or its Group of Companies shall be understood as neither given nor endorsed by PETRONAS or any of the companies within the Group.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...