Hi,
If your construction code is ASME,then WPS with Plate or pipe can be used for both in production joint.If there is no Impact test requirements,you can use the WPS with either group number.
Thanks & Regards,
(Karthik)
Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282
From: mithailal gupta <mrgupta_2007@yahoo.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Friday, November 11, 2011 3:47 PM
Subject: Re: [MW:12931] Preparation of WPS and PQR for GTAW and SMAW
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent: Friday, November 11, 2011 3:47 PM
Subject: Re: [MW:12931] Preparation of WPS and PQR for GTAW and SMAW
Dear Vikas
Many thanks for your input....but I am still not sure how to use both the material test specimen together as one is pipe and other is plate material (SA 516 Gr. 70 has different Group no. but P no. is same).
RGDS
M R Gupta
From: vikas shelke <vikas.shelke84@gmail.com>
To: materials-welding@googlegroups.com
Sent: Friday, 11 November 2011 1:28 PM
Subject: Re: [MW:12928] Preparation of WPS and PQR for GTAW and SMAW
To: materials-welding@googlegroups.com
Sent: Friday, 11 November 2011 1:28 PM
Subject: Re: [MW:12928] Preparation of WPS and PQR for GTAW and SMAW
Dear Mr. Gupta,
--
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
1) Only one WPS/PQR can qualify your range.
2) You can qualify the same using a 20 - 22 mm Plate coupon.
3) Filler to be used - ER 70S2 & E 7018 for SMAW.
4) You can qualify with Single -V Butt Joint.
On Fri, Nov 11, 2011 at 9:25 AM, MRG <mrgupta_2007@yahoo.com> wrote:
Dear All
I have to make a WPS and PQR for Pipe ASTM 106 Gr. B (P no. 1and Gr.
no.1) and Dishend SA 516 Gr. 70 (P no. 1 but Gr. no.2) both 40mm thk &
24" dia using GTAW Root and Hot Pass then SMAW for the remaining
passes as per Sec. IX of ASME.
Kindly give your input on below points.....
1) Is it possible to make only one WPS for the above processes?
2) What should be the joint design for both and also SA 516 Gr. 70 is
not available in pipe?
3) What should be the recommended filler rod and Electrode to be used?
4) What thickness of pipe to be used to qualify the above WPS so it
can for the production weld?
5) What should be the preheat temp and Interpass temp?
If you have any sample WPS and PQR for this then Pl do forward it to
me.
Looking forward for your reply.
RGDS
M R Gupta
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Regards,
Vikas Shelke,
+91-9881749268.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments