Re: [MW:12865] Welding Defect Photo

Other term commonly used for lack of penetration is suck back (in this case it may completely fuse at all face of the metal, but still happen lack of penetration). Lack of penetration is different than Lack of fusion. Some time we can see the weld metal fully penetrate through the root but there is some area at the roof face is not fuse well (this is called Lack of fusion).
 
From: Dindo <dindodelacruz@gmail.com>
To: materials-welding@googlegroups.com
Sent: Thursday, November 3, 2011 10:06 PM
Subject: Re: [MW:12859] Welding Defect Photo

There is a difference between the two. When I took the course for CSWIP 3.2, TWI explained it very well and how it was called by its name is what it really is.
 
Incomplete Penetration is when the root did not go through the the "land"
 
Lack of root fusion is when the weld went through the "land" but did not fused on the "land" in one side or both sides.
 


 
On Thu, Nov 3, 2011 at 7:15 AM, Morin, Darcy (Bantrel Management Services) <MorinD@bantrelmanagementservices.com> wrote:
Thank you very much for this resource.  It is very helpful. 
 
I notice what TWI describes as "lack of root fusion" and what ASME B31.3 describes as "incomplete penetration" are in fact one and the same.  
 
In normal service, a girth butt weld designed under ASME B31.3, a weld is allowed 38 mm of "incomplete penetration" for every 150 mm of weld. BUT zero "lack of fusion".  Many RT interpreters under ASME B31.3 confuse the 2 indications, leading to unnecessary rework and an artificially high repair rate.  Can any of our experts speak to this?
 
Warm regards,
 
Darcy Morin    

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Anil Hegde
Sent: Wednesday, November 2, 2011 11:24 AM
To: materials-welding@googlegroups.com
Cc: harryeng.09@gmail.com
Subject: Re: [MW:12831] Welding Defect Photo

Hope this will help you.


tc

On Wed, Nov 2, 2011 at 3:39 PM, Harry Patel <harryeng.09@gmail.com> wrote:
Dear Sirs,
 
Anybody have welding defect photo like incomplet fusion,incomplete penetration, root concavity in pipe.
 
I hope for your reply.
 
Thank you very much in advance.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
This e-mail and any attachments may contain confidential and
privileged information. If you are not the intended recipient,
please notify the sender immediately by return e-mail, delete
this e-mail and destroy any copies.

Any dissemination or use of this information by a person other
than the intended recipient is unauthorized and may be illegal.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...