As such hardness test for 316L is not required after or prior to hydrotest.
From: lassaad mokrani <lassaad.mokrani@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wednesday, 28 September 2011 2:37 PM
Subject: [MW:12565] HARDNESS MEASUREMENT MAP
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
To: materials-welding@googlegroups.com
Sent: Wednesday, 28 September 2011 2:37 PM
Subject: [MW:12565] HARDNESS MEASUREMENT MAP
Dear Experts,
--
Meilleures salutations
Mokrani Lassaad
00216 20 649 755
http://www.linkedin.com/pub/lassaad-mokrani/16/364/907
P Pensez environnement! N'imprimez ce mail que si c'est vraiment nécessaire
Please consider your environmental responsibility before printing this e-mail
This e-mail is confidential and it is intended only for the addressees. Any
review, dissemination, distribution, or copying of this message by persons
or entities other than the intended recipient is prohibited. If you have
received this e-mail in error, kindly notify us immediately by telephone or
e-mail and delete the message from your system. The sender does not accept
liability for any errors or omissions in the contents of this message which
may arise as a result of the e-mail transmission
-- We have completed sucessfully Hydrotest of our two SS 316L vessles.
For stress relieiving reasons, we have asked our supplier and since the beginning, to foresee some spot checks on hardness of the shells.
Now, is there any standard mapping/ number of points to be checked??
Logically, the more strained fiber is by the external surface of the shell, so which points to select or hardness testing??
Many thanks for a prompt reply
Regards,
Meilleures salutations
Mokrani Lassaad
00216 20 649 755
http://www.linkedin.com/pub/lassaad-mokrani/16/364/907
P Pensez environnement! N'imprimez ce mail que si c'est vraiment nécessaire
Please consider your environmental responsibility before printing this e-mail
This e-mail is confidential and it is intended only for the addressees. Any
review, dissemination, distribution, or copying of this message by persons
or entities other than the intended recipient is prohibited. If you have
received this e-mail in error, kindly notify us immediately by telephone or
e-mail and delete the message from your system. The sender does not accept
liability for any errors or omissions in the contents of this message which
may arise as a result of the e-mail transmission
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments