I am not sure but you can try this for an explanation.

As per ASME sec-VIII div.1 simulation PWHT of P1 material is not required,

There is another parameter(Larsen miller) to identify the equivallent  heat treatment for a material,in which on the basis of TC you can calculate Tp for Min and Max heat treatment temp and time. Now calculate the Tp for actual heat treatment and prove that your actual Tp is within the range. 

Tempering parameter (TP) : (Larsen Miller parameter)

 

Parameter for calculating equivalent heat treatment

Conditions as follows:

 

TP = (T+273)(20+log10t)×10-3

 

Where T = holding temperature (°C), t = time (hours)


This is not acceptable as per code but technically you can give additional clarification along with test coupon of same grade.


Regards,

Vaibhav Joshi



On Mon, Sep 12, 2011 at 11:45 AM, Karthik <karthik6684@yahoo.com> wrote:
Hi,
Was this vessel installed at Australia or Newzealand? Also please verify your design calculation,whether the vessel was designed to AS1210 or ASME. If the vessel designed to AS1210 and installed at Australia then you have to follow AS4458(Construction Code).
Or if the vessel designed to ASME,then you can inform to your client that we have followed ASME for construction too.
Even if the customer stick on AS4458 requirement,you can inform them that we will do SR and Mechanical test on a sample piece with the same Material grade to prove that the mechanical properties are within the code requirements.This is only the option if the customer need for AS4458 requirements.
Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Mon, 9/12/11, murugesan jeyaraman <jmurugesan@gmail.com> wrote:

From: murugesan jeyaraman <jmurugesan@gmail.com>
Subject: Re: [MW:12436] Need advise to clarrify client - Dish head stress relieving simulated PWHT test panelDate: Monday, September 12, 2011, 11:58 AM


Yes, as per Drawing we have to comply with ASME and Australian standard

On Fri, Sep 9, 2011 at 4:17 PM, Karthik <karthik6684@yahoo.com> wrote:
Hi,
Did u use 3 Codes for your vessel construction? Strange. and how it is possible to use 3 codes in one vessel construction?...
Pls.verify your design and drawing for the Construction Code.If it is specify ASME Sec.VIII-Div.1 .,then you can reply to your customer that you have followed ASME.

Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Fri, 9/9/11, murugesan jeyaraman <jmurugesan@gmail.com> wrote:

From: murugesan jeyaraman <jmurugesan@gmail.com>
Subject: [MW:12389] Need advise to clarrify client - Dish head stress relieving simulated PWHT test panel
To: materials-welding@googlegroups.com
Date: Friday, September 9, 2011, 2:29 PM

Dear Friends
 
Please offer me your suggestion how we can settle the following case.
 
We fabricated and supplied one pressure vessel to one of our client two years back. Now only they have reviewed our documents and come back with following observations.
 
Code of construction is ASME VIII Div 1 and AS1210 and AS4458, Material SA 516 Gr 70, thickness 30 mm,
 
Our vessel dish head is Stress relieved as per ASME viii Div 1 code requirement, but we have not done any simulated PWHT test panel for this stress relieve treatment.
 
 as per AS 4458, Unless any mechanical  test is done to prove Stress relieved components are restored to their original material properties, normalising is the preferered heat treatment for cold formed components.
 
It is obvious from above that either we have to do SR with Simulated PWHT test panel or Normalising of dished head.
 
Actually we have overlooked AS 4458, so we have only done SR without PWHT test panels, so no mechanical testing was done.
 
At this stage we cannot do normalising as plant is already running.
 
At this stage, we do no have stock of same heat number plate.
 
Please suggest how we can answer this observation.
 
Can we say we have overlooked AS and SR done as per ASME Viii Div 1 as a normal practice in South east asia.
 
We hve not done any Hardness test  being carbon steel material.
 
Thanks
 
 Murugesan
 
 
 
 
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...