Re: [MW:12385] RE: 12370] Hardness in Tube to tube sheet welding

Dear,

Preheat is one of the good tool to control an hardness try using 150 C -200 C preheat. that may work for you. Moreover there are some special NACE grade of consumables available.

Regards,
Vaibav Joshi

On Thu, Sep 8, 2011 at 6:32 PM, Abid Inamdar <abidinamdartech@gmail.com> wrote:
Ok, the details are:
Tube sheet material is HIC SA516, Thickness: 1" and 1.5" with J groove.
Tube material SA210 with 2.5 and 3.00mm thick.
Stength weld (first run with out filler wire and second run with filler ER70s2, 2.5mm dia filler.
Header: Closed type and welding from Plug holes.
 

I hope the details are OK.
 
regards
Abid
On Thu, Sep 8, 2011 at 12:08 PM, Pieper QSI <pieper-qsi@kpnmail.nl> wrote:
Dear Sir,

Before any member can give a useful reply some additional information is
required, such material kind and wall thickness of tube and tube sheet. Also
design code may be helpful to offer a solution.
Without this it's only a guess.

Met vriendelijke groeten / Best Regards

Herman Pieper

Pieper Quality Support & Inspection
Phone: +31 (0)521 380083
Fax:     +31 (0)84 7539225
Cell:     +31 (0)6 51691215
www.pieper-qsi.nl

-----Oorspronkelijk bericht-----
Van: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] Namens Inamdar
Verzonden: donderdag 8 september 2011 7:05
Aan: Materials & Welding
Onderwerp: [MW:12370] Hardness in Tube to tube sheet welding

I seek some guidance in the above.
Our Hardness for tube to tube sheet welding is coming above 250HV and the
desired value is 210 Avg.
Can some body explain me the below:
1) Which code clealy specifies the maximum acceptable value of hardness in
TTS welding.?
2) How to control the hardness without PWHT in TTS welding?

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and
meant for educational purposes only, Users must take their own decisions
w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Blog Archive