Skip to main content

Re: [MW:11766] Impact value in HAZ

Any mode of transfer that gives you less heat input is better in these applications.
Spray transfer in GMAW normally gives better HAZ impact values...
I have tried spray transfer in many cases that PQR tests failed the specimens welded with short-circuit mode of transfer... It works...!!!

But whatever you do be sure to deposit the welds so that they "temper" the layer underneath, this way you can get ood results specially in repair-welding.

use dressing technique for cap run or deposit another layer atop the cap run and then remove by grinding...

PWHT improves HAZ toughness but normally it's useful for thicknesses above 1"


Ramin  Kondori
   QC/Welding Engineer 
         IWE AT 0070
   



On Sat, Jul 16, 2011 at 3:43 PM, yusufkhan pathan <yusufkhanp97@gmail.com> wrote:
Dear sandeep,
 
However as mentioned by Dinesh, voltage, current & travel speed as the important factors afftecting the heat input.
as per my past experience related to SMAW we used to control these factors by increasing the travel speed thereby resulting in good impact values. I am not sure about GMAW, whether this method can be applicable.
Another factor which effects the energy value is the choice of consumables.
 

Regrads,

Yusufkhan. M. Pathan

Engineer-Quality

Air Liquide Engg (IND) Pvt.Ltd.

Email to : yusufkhan.pathan@airliquide.com

Cell:(+91) 8008804165



 
On Wed, Jul 6, 2011 at 12:29 PM, sandy <sandeepdhiman63@gmail.com> wrote:
Dear All
How we can get better impact values in HAZ with GMAW process in non
alloyed carbon steel?
like with multi pass welding.
Please provide your valuable ideas.

Regards
Sandeep Kumar

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...