Dear All,

 

This is just my view and my experience.

 

If the weld bead width (weaving) is more

Then the profile of the weld bead will become concave at the center of the weld, and this type of shape is not suitable / recommendable for any of the Coating systems.

Because air will entrap in that location at the time of Joint coating and will effect adversely on the coating system.

All this phenomena is because of more width of the weld bead, and as per practice condition and previous experiences 3 times of the electrode dia weaving bead will not produce such kind of concaveness.

Hence this practice has implemented in welding – Especially in Coating required pipelines(Cross country / Onshore / Offshore / Subsea)

Engineers who had worked in pipelines will treat this is a major point and started putting this general statement in WPS – Which in not that much big Issue and will not affect any parameter

 

Thanks & Regards

 

Lakshman kumar.B | Manager - QA/QC | LANCO  INFRATECH LIMITED
www.lancogroup.com

Go Green |The future will thank you

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ahmed Husain
Sent: Tuesday, April 05, 2011 4:03 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:10599] Weaving

 

Dear Mr Rogers,

 

First, If weaving has so critical effect on welding, then why its limitation is not stated in Codes.

Second, on what basis, anyone decide that weaving above 3 times of electode dia will affect the grain structure and impact value of weld metal, and below that will produce satisfactory weld metal property.

Third, different material have different impact toughness requirement, but generally  WPS for all materials requires weaving limitaion. 
 

Ahmed Husain
Mob-0547170325

 

 


From: Geoff Rogers <gbr476@gmail.com>
To: materials-welding@googlegroups.com
Sent: Tue, April 5, 2011 12:44:22 PM
Subject: Re: [MW:10598] Weaving

The amount of weaving directly affects the heat input since the wider the weave the slower the travel speed.  With a slower travel speed the greater the heat input which will affect the weld and HAZ grain structure. This typically leads to lower impact toughness values and increased hardness.  Typically the tensile strength is not affected by the extent of weave.  Also, the width of the weave affects how well the weld pool is protected by the shielding and how well the weld metal will fuse to the base metal.  A max weave of 3 times electrode diameter for SMAW and 5mm for GMAW is typically specified since it produces the best overall weld quality and mechanical properties for the productivity achieved.

Geoff Rogers
Welding Engineer
Houston, TX

On Tue, Apr 5, 2011 at 2:42 AM, Ahmed Husain <ahmraha@yahoo.com> wrote:

Dear All,

 

Almost all SMAW WPS prepared in accordance to ASME IX, I have seen, it specify maximum weaving 3 times the electrode dia. But I am unable to co-relate this WPS requirement to any ASME code or Client (ARAMCO) requirement . If weaving 3 times electrode dia is not stated in ASME codes, then why does it is mentioned in WPS?

 

Kindly share some information on this subject.

 


 

Ahmed Husain
Mob-0547170325

 

 


From: ramu ramalingam <ramu.srivi@gmail.com>

Sent: Fri, April 1, 2011 9:49:05 AM
Subject: Re: [MW:10554] Weaving

 

Hai,

 

If they want to weave more than 3 times of electrode/filler wire dia, better to make new WPS and proof all the necessary requirement to meet with old WPS.

 

Because,when we weave more, in production weld that time heat input will be increased and  its fail in tenstile test. The heat inputput  should not be more than 3 KJ/min for each process.

Regards,

RR

 

On Wed, Mar 23, 2011 at 11:31 PM, Sampath Kumar <skthatham@gmail.com> wrote:

Dear Friends,

 

WPS says the weaving is allowed/permitted 3times the diameter of the electrode.Please tell me wheather we can allow if the weaving is more than the allowable limit.If it can be allowed.What is the reasons and on what basis it is allowed?If it can not/should not be allowed.Why and what is the reasons?

 

My opinion is that it should not be allowed.[1]Because it deviates from the WPS.[2]properties may vary because of the excess heat In put due to excess weaving.

 

The contractor is of opinion that they will change the WPS to suit excess weaving.It is not an essential variable,hence it can be allowed.To substantiate their claim they say they will change the WPS and they will perform Hardness Test to prove that the properties were not changed.

With Best Regards

Sampath

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...