Skip to main content

Re: [MW:9096] PWHT Requirement For CRO

Dear sir,

Thanks for your replay

But what about the notes in UCS-56 2 (c) 5
that is if preheat (95 deg c) is there PWHT is not mandatory for thickness greater than 33mm

On Wed, Jan 5, 2011 at 1:04 PM, Karthik <karthik6684@yahoo.com> wrote:
Hi,
Yes.You should do PWHT of SA516 with CRO as per ASME Sec,VIII,DIV 1,UCL34.Please find below the extraction.
UCL 34
(a) Vessels or parts of vessels constructed of base material
with corrosion resistant integral or weld metal overlay
cladding or applied corrosion resistant lining material shall
be postweld heat treated when the base material is required
to be postweld heat treated. In applying these rules, the
determining thickness shall be the thickness of the base
material.
When the thickness of the base material requires postweld
heat treatment, it shall be performed after the application
of corrosion resistant weld metal overlay cladding or
applied corrosion resistant lining unless exempted by the
Notes of Table UCS-56.
(b) Vessels or parts of vessels constructed of chromium
stainless steel integral or weld metal overlay cladding and
those lined with chromium stainless steel applied linings
shall be postweld heat treated in all thicknesses, except
vessels that are integrally clad or lined with Type 405 or
Type 410S and welded with an austenitic electrode or nonair-
hardening nickel–chromium–iron electrode need not be
postweld heat treated unless required by (a) above.

Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Wed, 1/5/11, rinshad abdul rahman <rinshad043@gmail.com> wrote:

From: rinshad abdul rahman <rinshad043@gmail.com>
Subject: [MW:9091] PWHT Requirement For CRO
To: materials-welding@googlegroups.com
Date: Wednesday, January 5, 2011, 3:49 PM

Dear all,

 I just want to know that whether PWHT is required for CRO on SA516 Gr. 70 (60  mm thick) on the same part we need do SMAW+SAW weld with 60 mm nominal size (construction is as per ASME BPV SEC VIII DIV 1)

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...