Dear Naushad,
Deposit ENP thickness can be measured by using sample coupons along with the parts, by means of weigh plate weigh method as per ASTM B733,para 9.3.5
If necessary, a microscopic examination of the cross section of the coupons can be carried out as per ASTM B733 para
9.3.1
If thickness is in the range of 25- 75 microns, i would suggest you to go for microscopic examination that shall be:-
Regards,
Manpreet Singh
Welding Engineer
Spiecapag
On Tue, 30 Nov 2010 21:25:21 +0530 Harish Kannepalliwrote
>
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Deposit ENP thickness can be measured by using sample coupons along with the parts, by means of weigh plate weigh method as per ASTM B733,para 9.3.5
If necessary, a microscopic examination of the cross section of the coupons can be carried out as per ASTM B733 para
9.3.1
If thickness is in the range of 25- 75 microns, i would suggest you to go for microscopic examination that shall be:-
Direct measurement by micrometer on coupons before and after the plating.
Acceptance: parts shall be considered non-conforming if one
measurement fails to meet the specified tolerance.
Regards,
Manpreet Singh
Welding Engineer
Spiecapag
On Tue, 30 Nov 2010 21:25:21 +0530 Harish Kannepalli
>
You can go for wet chemical method like weight loss method for better results.
>
>
>
>--
>
>
-- >
>
2010/11/30 Noushad cp <ncp.clt@gmail.com>
>
>
Dear All,--
>
>How to measure Electroless Nickel Plating (Coating) ?i would like to know the Instrument which is use for ENP Measurement.
>
>Thanks and Regards,
>
>Noushad
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
>
>--
>
regards,
Harish.
>
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments