Skip to main content

Re: [MW:8272] Welding of Gr.11 material with Gr. 91 material.

Dear Vikas :

If design allows, you may try to add T22 material as bridge material among T91 to T11. I have try this approach before and quite happy with the result.
Yet, discuss with your engineering team first.

regards
Bonardo


From: Vikas Bhandari <vikas.bhandari349@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wed, 10 November, 2010 3:44:08 PM
Subject: Re: [MW:8183] Welding of Gr.11 material with Gr. 91 material.

Dear all

As per SEc II part A, 
PWHT for T11 :650 C
PWHT for T91:730-800 C

If the same situation is met in other materials, I was wondering how to find out the final heat treatment temperature and how to bridge the gap of heat treatment requirement between the two different materials.
Would taking out an approximate average of the requirements suffice? 

On Wed, Nov 10, 2010 at 3:11 AM, Prakash Hegde <pb.hegde@yahoo.com> wrote:
Gr11 to Gr91 being discimilar joint
 
PWHT temperature of 745C is high for Gr11 material and you may land up with not meeting the Physical properties . Using equivalent consumables for Gr 11 material (B2 Type) you may require to reduce the PWHT temp to 700C  and accordingly qualify the PQR
 
Regards
Hegde P.B.
09714714803

 


From: siva chidambaram <mechsivachidambaram@gmail.com>
To: materials-welding@googlegroups.com
Sent: Tue, 9 November, 2010 10:32:52 PM
Subject: [MW:8171] Welding of Gr.11 material with Gr. 91 material.

Dear all,

I have a doubt in welding of Gr.11 material with Gr. 91 material.
The details are as follow:
Joint Type: Fillet weld
Material; SA 213 Gr. T91 with SA 213 Gr. T11
Process: GTAW & Also in SMAW
Consumable: For GTAW: ER 80S-B2 & for SMAW : E8018-B2
Preheating: 200°C
PWHT: 745° ± 15°C

In this welding, Whether there will be any metallurgical problem. If so what is the alternate for it.

M.Sivachidambaram




--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...