Hi,

For Sensitisation to occur in SS, carbon is required.

Grade 316L, the low carbon version of 316 is immune from
sensitisation (grain boundary carbide precipitation).

So, there will be no problem if you do PWHT at temperature 600 DEG
CELSIUS for SS316L.

Regrads

Prabhakar,
BV


On 04/11/2010, Prabhakar Raj <prabhakarmet@gmail.com> wrote:
> Hi,
>
> Grade 316L, the low carbon version of 316 is immune from
> sensitisation (grain boundary carbide precipitation).
>
> So, there will be no problem if you do PWHT at temperature 600 DEG
> CELSIUS for SS316L.
>
> Regrads
>
> Prabhakar,
> BV
>
> On 03/11/2010, Kathalingam Babu <kathalingam.qaqc@ppl.com.sg> wrote:
>> Hi
>>
>> Apologies for the incorrect spelling of "Sensitization"
>>
>> Regards
>>
>> K.Babu
>> Singapore
>>
>> ----- Original Message -----
>> From: Kathalingam Babu
>> To: materials-welding@googlegroups.com
>> Sent: Wednesday, November 03, 2010 5:32 PM
>> Subject: Re: additional detail[MW:8044] effect of PWHT Temperature at
>> 600
>> DEG CELSISIUS ON SS 316L
>>
>>
>> Hi Karthik
>>
>> Yes there is more chances for the sensitation , if you SR at the
>> sensitation temp. range after forming.
>>
>> Cold forming of SS316L is generally SR Iis not required, as it is
>> having
>> good ductility and formability.
>>
>> Also we need to have the Capcity of Equipment is higher than what we
>> using
>> for the SS304.
>>
>> Upto 8 mm thk, very well formed , with generally available equipments.
>>
>> Regards
>>
>> K.Babu
>> Singapore
>>
>>
>> ---- Original Message -----
>> From: Karthik
>> To: materials-welding@googlegroups.com
>> Sent: Wednesday, November 03, 2010 4:17 PM
>> Subject: Re: additional detail[MW:8043] effect of PWHT Temperature at
>> 600 DEG CELSISIUS ON SS 316L
>>
>>
>> hI,
>>
>> I agree with Mr.Babu.But as far as i know Sensitation
>> Temp.range
>> for SS316L is 450 to 600 degrees.
>>
>> My doubt is If Sensitation Temp.range for SS316L is of 600 to
>> 850
>> means,In case of doing Stress reliving(some times after forming needed)
>> around 850 degrees will it get sensitised?
>>
>>
>>
>>
>> Thanks & Regards,
>>
>>
>>
>> (Karthik)
>>
>>
>>
>> Karthikeyan.S
>> QA/QC Manager
>> Getabec Energy Co.,Ltd.
>> 379,Moo6,Soi8,Nikhomphatana,
>> Rayong-21180,
>> Thailand.
>> Phone: 0066 38 897035-8 (Off)
>> Fax: 0066 38 897034
>> Hand Phone: 0066 892512282
>>
>>
>> --- On Wed, 11/3/10, Kathalingam Babu
>> <kathalingam.qaqc@ppl.com.sg> wrote:
>>
>>
>> From: Kathalingam Babu <kathalingam.qaqc@ppl.com.sg>
>> Subject: Re: additional detail[MW:8039] effect of PWHT
>> Temperature at 600 DEG CELSISIUS ON SS 316L
>> To: materials-welding@googlegroups.com
>> Date: Wednesday, November 3, 2010, 3:02 PM
>>
>>
>> Hi
>>
>> SS 316L doesn't have any Stabilizing elements. Since the
>> lower
>> percentage of carbon , the tendency of Cr Carbide formation is less.
>>
>> Sensitation temperature range for the SS316 is typically in
>> the
>> range of 600~850 deg. cel.
>>
>> If you want to do PWHT, you may do less than 575 deg. cel.
>> and
>> increase the soaking time accordingly.
>>
>> In my opinion, I'll not recommend for PWHT with internals.
>>
>> Regards,
>>
>> K.Babu
>> Singapore
>>
>>
>> ----- Original Message -----
>> From: Karthik
>> To: materials-welding@googlegroups.com
>> Sent: Wednesday, November 03, 2010 3:45 PM
>> Subject: Re: additional detail[MW:8038] effect of PWHT
>> Temperature at 600 DEG CELSISIUS ON SS 316L
>>
>>
>> hi,
>>
>> If you PWHT with Austenitic SS (SS316) internal
>> sensitation happened at 450 to 600 degrees which will reduce the
>> corrosion
>> resistance of SS316(chromium becomes chromium carbide).
>>
>>
>> But in your case it is SS316L ,for this it may PWHT
>> since 'L" grade has stabilising elements like Ti,Cb,Nb which will help to
>> reduce the sensitation.
>>
>> So if you are not ready to dismantle the internal for
>> PWHT,you may go with SS316L internal for PWHT.
>>
>>
>> Thanks & Regards,
>>
>>
>>
>> (Karthik)
>>
>>
>>
>> Karthikeyan.S
>> QA/QC Manager
>> Getabec Energy Co.,Ltd.
>> 379,Moo6,Soi8,Nikhomphatana,
>> Rayong-21180,
>> Thailand.
>> Phone: 0066 38 897035-8 (Off)
>> Fax: 0066 38 897034
>> Hand Phone: 0066 892512282
>>
>>
>> --- On Wed, 11/3/10, asad azmi
>> <azmiasadayub@gmail.com>
>> wrote:
>>
>>
>> From: asad azmi <azmiasadayub@gmail.com>
>> Subject: [MW:8034] effect of PWHT Temperature at
>> 600
>> DEG CELSISIUS ON SS 316L
>> To: materials-welding@googlegroups.com
>> Date: Wednesday, November 3, 2010, 1:44 PM
>>
>>
>> Dear All,
>>
>> Greetings.
>>
>> Contractor is doing PWHT of the Carbon Steel Vessel
>> along with SS316L INTERNALS ( BEAMS, CHANNELS) Bolted with the Vessel.
>> PWHT temperature is 600 DEG CELSIUS.
>>
>> Pls suggest me whether it is allowed. what will be
>> the effect on mechanical proerties/corrosion ressiatnce proerties of SS
>> 316L becuase of the PWHT Temperature.
>>
>> Thanks in advance for your valuable suggestions.
>>
>> Regrads
>> --
>> To post to this group, send email to
>> materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are
>> members personel views and meant for educational purposes only, Users
>> must
>> take their own decisions w.r.t. applicable code/standard/contract
>> documents.
>>
>>
>> --
>> To post to this group, send email to
>> materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members
>> personel views and meant for educational purposes only, Users must take
>> their own decisions w.r.t. applicable code/standard/contract documents.
>>
>> --
>> To post to this group, send email to
>> materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members
>> personel
>> views and meant for educational purposes only, Users must take their own
>> decisions w.r.t. applicable code/standard/contract documents.
>>
>>
>>
>>
>> --
>> To post to this group, send email to
>> materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members personel
>> views
>> and meant for educational purposes only, Users must take their own
>> decisions
>> w.r.t. applicable code/standard/contract documents.
>>
>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members personel views
>> and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>>
>> --
>> To post to this group, send email to materials-welding@googlegroups.com
>> To unsubscribe from this group, send email to
>> materials-welding+unsubscribe@googlegroups.com
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>> The views expressed/exchnaged in this group are members personel views
>> and
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>>
>

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...