Skip to main content

RE: [MW:7416] use of E 6010 for fillet weld

You can, But why do you want to use E6010 for fillet?

Fillet welds when made with E6010 usually have a relatively flat weld face and have a rather coarse, unevenly spaced ripple.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Karthik
Sent: Thursday, October 07, 2010 1:17 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:7414] use of E 6010 for fillet weld

 

Hi,

Yes.You can use.

 

QW-451.4

 

FILLET WELDS QUALIFIED BY GROOVE-WELD TESTS

 

Thickness T of Test

Coupon (Plate or Pipe)                                                     Type and Number of Tests

as Welded                         Range Qualified                      Required

 

All groove tests                  All fillet sizes on all base         Fillet welds are qualified when

                                          metal thicknesses and all         the groove weld is qualified

                                         diameters                                  in accordance with either QW-451.1 or QW-451.2

 

 

Thanks & Regards,

 

(Karthik)

Karthikeyan.S

QA/QC Manager

Getabec Energy Co.,Ltd.

379,Moo6,Soi8,Nikhomphatana,

Rayong-21180,

Thailand.

Phone: 0066 38 897035-8 (Off)

Fax: 0066 38 897034

Hand Phone: 0066 892512282



--- On Thu, 10/7/10, asad azmi <azmiasadayub@gmail.com> wrote:


From: asad azmi <azmiasadayub@gmail.com>
Subject: [MW:7412] use of E 6010 for fillet weld
To: materials-welding@googlegroups.com
Date: Thursday, October 7, 2010, 1:38 PM

Dear All

 

Good Day.

 

 

I have WPS which was qualified using E6010 for Root pass and rest welding with E7018  for P1 Material of thickness 10mm.

 

 

Please inform me whether I can use above WPS for welding fillet weld  of 10 mm for P1( SA 36)  material using E6010 Electrode.

 

 

Thanks in advance for your valuable suggestions.

 

Best Regards

 

Asad Azmi

 

 


Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...