Hi Ganesh,

 

What’s the design/construction code ?, B-31.1 or Sec-I.

 

For Grade -91(Sec-IX-P-15E)  material you do not have the choice of performing PWHT at a lower temperature than what’s specified the design code. The recommended  PWHT temperature range for P-91 materials for electric utility applications are as follows:-

 

·         Section-I, Code- 730 Deg C minimum, 775 Deg C maximum

·         B-31.1 Piping Code- 730 Deg C minimum, 775 Deg C maximum

 

I would say the recommendation would be  to perform the PWHT again at the above specified range. This should be  in line PWHT temperature  followed for   WPS/PQR qualification. If the PQR was qualified with maximum time , any amount of time upwards of 90 minutes, there should not be any issues with meeting the nominal mechanical properties,following Re-Stress Relieving.

 

Otherwise it would be wise to verify the  tempering condition of the base metal in the mill and then to select the best PWHT cycle (time and temperature).

 

I do not want to be prejudiced or throw a smoke screen, if you do a goggle search on “failures of  P-91 steel” you’d come across some recent incidents. The following article from welding journal gives some food for thoughts. P-91 steel works under extremely demanding conditions, improper welding could be dangerous.

 

 

Thanks.  

 

 

Pradip Goswami, P.Eng

Welding & Metallurgical Engineer/Specialist

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ranjith Kumar .B
Sent: Tuesday, October 12, 2010 9:08 AM
To: materials-welding@googlegroups.com
Cc: 'Ganesan'
Subject: [MW:7505] PWHT

 

Dear Sirs,

 

We have Planned to Stress relive the Pipe butt joint of SA 335 Gr P91and Dia.323.9X33.3 at Soaking Temp:745°C ±10°C and soaking time:90mints. But by mistake while in process the operator has completed the Stress reliving at Soaking Temp:695°C ±10°C and soaking time:90mints.

 

For this can go to Re- stress reliving or can I accept as in condition(Request to guide me by mentioning the related standard) . I request any of us to guide me in this case to proceed further.

 

 

Thanks and Warm Regard’s,

 

K.GANESAN/QA&C,

 

 

 
 
 
-------------------------------------------
D F Power Systems Pvt Ltd, Bangalore, India
 
 
!-- Virus-Free Mail Using AntiVirus for PostMaster Enterprise & QuickHeal Engine --!

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

No comments:

Re: [MW:34913] Filler wire

E71T-1C  is Charpy Impact tested at -20degC E71T-1CJ is Charpy impact tested at -40degC. AWS Classification for FCAW is only a supplementary...