Re: Re: [MW:6926] Dilution cracking

for joining the dissimilar metals end microscopic structure is not only the issue but number of factors which play the role,some important are metallurgical stability of dissimilar metal composition and thermal expansion etc.

On Fri, 09 Jul 2010 13:04:46 +0530 wrote

Welding of stainless steel with carbon steel electrodes results in formation of martensite structure which is prone to cracking under stress or it may crack immediately during welding depending upon the welding conditions, thickness of the part being welded, deposition of consumable etc. But in actual practice, cracks do not come up always. Many a times, welders weld the stainless steel piping with carbon steel in order to avoid the need of purging and they successfully make the weld without any defects that can be picked up in radiography. They weld the root pass with carbon steel consumables and the rest of the welding is made in SS consumable.


However, welding of stainless steel with low alloy steel electrodes would definitely come up with cracking as it is more susceptible to cracking than carbon steel consumables. Same martensite structure formation would occur and LAS consumable being used without any preheating protocol would crack itself during welding mainly due to uncontrolled cooling.


Both of the situations can be seen visually during inspection and one can say that carbon steel or LAS consumable has been used but if gone un-inspected then one may not get it picked with radiography especially in the case of carbon steel consumable, however, LAS consumable has pretty higher chances of getting cracked and picked up.



 
On Thu, Jul 8, 2010 at 10:09 PM, Ankur Mande wrote:

Hello friends,

I have just joined this wonderful & group with "active members". I

have one query. Please let me know as to why we observe cracking when
carbon / low alloy steel is accidently welded on stainless steel. If
any body has any backup or paper related to this, request you to post
it.


Regards,

Ankur Mande.
09925027848

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com

For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Never bend my head infront of anyone other than GOD the almighty.




--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>


Thanks & regards,


MOHIT SHARMA
ENGINEER (PRODUCTION)
ISGEC │ YAMUNANAGAR│HARYANA
+91 9034868324
Email: mohit104@gmail.com

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...