Skip to main content

RE: [MW:7163] Welder Qualification on WPS with PWHT

Hi Karthik,

 

If I follow table 451.1 of ASME IX, it will give the WPS a minimum thickness of 4.8mm.

 

The WPS is with PWHT procedures, then the minimum thickness of 4.8 mm would not be subjected to PWHT as per table 331.1.1 of ASME B31.1. Therefore, logically you can not indicate 4.8mm as the minimum thickness on a WPS with PWHT procedure.

And because the WPS is with PWHT procedure, you can only use this procedure on welding materials that would be subjected to PWHT, and as per table 331.1.1 of ASME B31.1, the minimum thickness is 20mm.

 

What do you think?

 

Again thanks for your reply.

 

 

Cheers,

 

Larry

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Karthik
Sent: Thursday, 23 September 2010 1:18 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:7159] Welder Qualification on WPS with PWHT

 

Hi,

WPS/PQR thickness qualifications follow Sec.IX.Table 331.1.1. of B31.3 -requirements of Heat treatment.It is apply during PWHT of PQR and production welding.

For welder Qualification No need to do PWHT,Because it is not an essential variable for Welder Qualifications.

 

Thanks & regards,

 

(Karthik)

Karthikeyan.S

QA/QC Manager

Getabec Energy Co.,Ltd.

379,Moo6,Soi8,Nikhomphatana,

Rayong-21180,

Thailand.

Phone: 0066 38 897035-8 (Off)

Fax: 0066 38 897034

Hand Phone: 0066 892512282



--- On Thu, 9/23/10, Larry <quality@unieng.com.au> wrote:


From: Larry <quality@unieng.com.au>
Subject: [MW:7149] Welder Qualification on WPS with PWHT
To: materials-welding@googlegroups.com
Date: Thursday, September 23, 2010, 8:33 AM

Hi There,

 

I’m developing a WPS with the following criteria:

 

Welding Code: ASME IX

Construction Code: ASME B31.3

 

Material: ASTM A333 / API 5L

Thickness: 44.45mm; 400 NB pipe

Preheat: 79°C

PWHT: 593°C - 649°C as per table 331.1.1 of ASME B31.1

 

My question, is what is the thickness range, should I follow table 331.1.1 of ASME B31.1 for the minimum thickness, and table QW-451.1 of ASME IX for the maximum thickness?

 

Assuming all the necessary test on the coupon for the PQR have passed, and we need to do some welder qualification on the same WPS, do we need to do PWHT on the test coupon?

 

Thank you in advance.

 

 

Cheers,

 

Larry

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...