Re: [MW:7103] F-No&A-No of ERNiCrMo-3

Dear Raghuram sir,
 
I have reviewed my WPS and the following values observed.
 

Specification (SFA)  :  A 5.14(GTAW)

AWS classification   :  ER-NiCrMo-3(GTAW)

Trade Name            :  Thermanit625(GTAW)
 
 Filler metal product form : Solid (GTAW) 
 
Chemical composition in % for GTAW: C-0.008%, Si-0.06%, Mn-0.02%,Cr-22.32%,
Mo-8.93%, Nb-3.53%, Ni-64.10%,Fe-0.439%,P-0.001%,S-0.001%,Cu-0.039%,Ti-0.181% &Al-0.127%
 
 
Dear Karthik Sir,
 
Thank you for the correction,I had mistakenly typed QW.422 instead of QW.442
 
I have reviewed ASME QW.422 'A' No. section and couldn't find any matching chemistry with above mentioned chemical composition.
 
In this case,In the A-No column of WPS, what I have to write? N/A or Nil?
 
 
 
Regards,
 
 
Limesh

 



On Mon, Sep 20, 2010 at 11:26 AM, Karthik <karthik6684@yahoo.com> wrote:

Hi,

P.Number and F number are different and the numbers cannot be same and substituted.

For ERNiCrMo-3 F-Number is 43. For A number You can check with the QW-442 along with your Filler metal certificate to compare the chemical composition.Since it is a nickel based alloy,you check with the composition of A number 10 requirments.

 

Pls.find below the extraction of ASME appropriate sections. 

 

QW-404.37

A change in the composition of the deposited

weld metal from one A-Number in table QW-442 to

65

any other A-Number, or to an analysis not listed in the table.

Each AWS classification of A-No. 8 or A-No. 9 analysis of

table QW-442, or each nonferrous alloy in table QW-432,

shall require separate WPS qualification. A-Numbers

QW-404.5

(Applicable only to ferrous metals.) A

change in the chemical composition of the weld deposit

from one A-Number to any other A-Number in table

QW-442. Qualification with A-No. 1 shall qualify for

A-No. 2 and vice versa.

The weld metal chemical composition may be determined

by any of the following:

(a)

For all welding processes—from the chemical analysis

of the weld deposit taken from the procedure qualification

test coupon.

(b)

For SMAW, GTAW, and PAW — from the chemical

analysis of the weld deposit prepared according to the

filler metal specification, or from the chemical composition

as reported either in the filler metal specification or the

manufacturer's or supplier's certificate of compliance.


Thanks & Regards,
 
(Karthik)
Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Sat, 9/18/10, limesh M <limesh78@gmail.com> wrote:

From: limesh M <limesh78@gmail.com>
Subject: [MW:7073] F-No&A-No of ERNiCrMo-3
To: materials-welding@googlegroups.com
Date: Saturday, September 18, 2010, 8:08 PM


Dear All,
 
I want to prepare a WPS for ,
 
material ASTM B 423 (P No-45).
 
Process - GTAW
Construction Code - ASME B31.3
Welding Code - ASME BPV SEC IX
 
What is the F - No. of ERNiCrMo-3?  43 or 45?One of the  WPS in my hand says 45 !!!
I have reviewed ASME BPV SEC IX QW 432,F-No. section and found that 43.Now I need clarification from experts,which one is correct 43 or 45?
 
What is the A - No. of ERNiCrMo-3? I have reviewed QW 422 A-Numbers section,but couldn't find.
 
Is there any condition that P- no. and F- no. shall be same?
 
Seniors, I need your help on this issue.
 
 
Regards,
 
Limesh
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...