Re: [MW:7101] Re: TUBE TO TUBE SHEET EXPANSION

Have a look also in the UHX part of ASME BPVC VIII div 1


----- Original Message -----
From: "M. Ali" [mali5286@gmail.com]
Sent: 19/09/2010 23:57 MST
To: "Materials & Welding" <materials-welding@googlegroups.com>
Subject: [MW:7100] Re: TUBE TO TUBE SHEET EXPANSION

Dear Manoj,

You can find the required information from API 660, (9.10) Tube-to-
tubesheet joints. The content is given as allowable tube wall
thickness reduction of roller expanded tube to tubesheet joints.
Furthermore, you can tell us what material you are using for the
percentages

Regards,
Muhammad Ali
M.E. Mechanical, CSWIP 3.1
Executive Engineer, Inspection
PRL

On Sep 20, 9:24 am, Karthik <karthik6...@yahoo.com> wrote:
> Hi,
> Please find below the formula for tube expansion percentage.With this you can fix the max.allowable expansion percentage in relate to the thickness of the tube after expansion. also you can find the thickness of the tube after expansion by using this formuls(Tube ID after expansion-Tube OD / 2).In no case it will not be less than the design thickness of the tube.
> The tube longitudinal and compressive stress shall be calculated  by TEMA RCB7.23 or 7.24.
>  
> Formula.
> K = ((d2-d1) - (H-D))/2T X 100%
>  
> d2 = (H-2T+(Kx2T)/100)
>  
> Pls.see the attached file of sample calculation sheet.In this sheet you can input your datas and you will get the thickness reduction and tube ID after expansion.
> You can fix the K from 3% to 15% or what will be the minimum and maximum expansion percentage you fix.
>  
> Where,
> K-Expansion percentage,decrement of tube thickness
> T-Tube wall thickness
> d1-Inside diameter of the tube before expanding
> d2-Inside diameter of the tube after expanding
> D-outside diameter of the tube
> H-Inside diameter of the tube sheet hole
>  
> Thanks & Regards,
>  
> (karthik)
>  
> You can just make this in an exel sheet
>
> Karthikeyan.S
> QA/QC Manager
> Getabec Energy Co.,Ltd.
> 379,Moo6,Soi8,Nikhomphatana,
> Rayong-21180,
> Thailand.
> Phone: 0066 38 897035-8 (Off)
> Fax: 0066 38 897034
> Hand Phone: 0066 892512282
>
> --- On Sun, 9/19/10, manoj john <manojac...@gmail.com> wrote:
>
> From: manoj john <manojac...@gmail.com>
> Subject: [MW:7094] TUBE TO TUBE SHEET EXPANSION
> To: materials-welding@googlegroups.com
> Date: Sunday, September 19, 2010, 3:29 PM
>
> Dear All,
>  
> I have to do tube to tube sheet expansion.  This is as per TEMA and joint is double groove full expansion.  My question is from where i can get a reference from the code for the percentage of expansion.
>  
> Thanks in advance.
>  
> Best Regards.
> Manoj.
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
> For more options, visit this group's bolg athttp://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
>  Calculation sheet.xlsx
> 14KViewDownload

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...