Skip to main content

Re: [MW:6892] Storage conditions of E 7018 & Conflicts in it.

Hermetically sealed package : It's not vaccum packed and it is prone to absorb moisture. The extenet of moisture absorption over a period of time is given on the packing or on the consumbale data sheet / guide book. The recommnedation generally given by manufacturer is to bake and hold prior to use. One of the reason why baking is recommended is that, consumbales are stored in the manufacturers/traders warehouse for a long period and chances of moisture absorption is there.
 
Generall practice in industries:
 
1. Baking  of consumables for certain duration of time shall be done after removing from packing (Except for vaccum packing) as recommended by consumable manufactureres.
Note: Some Manufactureres also recommend that if consumbales are stored in controlled humidity and temperature atmosphere, then baking is not required and consumbales can directly be transferred in holding ovens. (Generally 120 - 150 deg. cent).
 
2. After baking, Holding of consumables in holding oven priro to use.
Note: Code only suggest / recommend the baking & holding conditions. Manufatureres recommendation must be followed.
 
There is a misunderstanding at your end . Please refer Table 3 in SFA 5.1 once again. It recommends the holding upto 140 deg.cent. and for baking 260 to 425 deg.cent for E7018.
 
3. If quivers are having analaog/ digital meter. It can be used as a holding ovens for the site. However, make sure that they are calibrated regularly. Generally, there are seperate holding ovens in which the electrodes are holded from which welders get the consumbales issued in quivers for use for certain duration (Approx 4 hrs). In this case, only ovens are required to be calibrated and not the quivers.
 
I hope your queries are cleared.
 
 
Dokku Ajay Kumar



From: kianoosh zarrin naghsh <kzarrinnaghsh@yahoo.com>
To: materials-welding@googlegroups.com
Sent: Sun, September 5, 2010 1:27:23 PM
Subject: Re: [MW:6872] Storage conditions of E 7018 & Conflicts in it.

Dear Srinivas,

There is different from the backing of electrode and the holding of electrode. Backing is done when its container is opened or the electrode is removed from its container, but holding the electrode is done immediately after removing the electrode from sealed container or when the electrode is backed.

Usually the backing is done in large oven, but the holding is done in portable oven for welders.

Low-hydrogen electrodes for shielded metal arc welding conforming to SFA-5.1 and SFA-5.5 shall be purchased in hermetically-sealed containers or shall be dried at least 1 hr at temperatures between 120 and 150 before being used. Electrodes shall be dried prior to use if the hermetically-sealed container shows evidence of damage. Immediately after the opening of the hermetically-sealed container or removal of the electrodes from the drying oven, electrodes shall be stored in ovens held at a temperature of at least 120°C. Electrodes that are not used within 1/2 hr after the opening of the hermetically-sealed container or removal of the electrodes from a drying or storage oven shall be dried as specified above before use unless evidence is presented which indicates that the brand of electrode used may be exposed for a longer period of time without exceeding the maximum moisture requirement.

Hermetically-sealed is equal to a container that protected, sealed and tightened from moisture, humid, water and … .

The backing temperature for A5.5 E7018 electrodes classifications is 250-400, but for A5.1 E7018 electrodes classifications is 120-150 in brands.

 

 Be Happy!

--- On Sat, 9/4/10, Srinivas Engr <srinivas.gmsrini@gmail.com> wrote:


From: Srinivas Engr <srinivas.gmsrini@gmail.com>
Subject: [MW:6861] Storage conditions of E 7018 & Conflicts in it.
To: "Materials & Welding" <materials-welding@googlegroups.com>
Date: Saturday, September 4, 2010, 2:10 AM

Dear all,

I am in confussion?

What's called hermetically sealed packages?
According ASME section 2 c SFA 5.1, Table A3,
for E 7018, its says 140degree Celsius is enough for backing oven
conditions, when its removed from packages.
but some manafatures says 300-350 celsius.

according to Table A3, we can use after baking in holding oven by 140
celsius & with quivers in site. am i right?

Is it correct or not?

When E7018 is expsoed to air, then only we have to baking to 300 - 350
celsius according table A3.

is any conflict in this? r any wrong in this?

Pl clear me...

Thanks
Srinivas

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...