Re: [MW:6840] tempering temperature of P4 material

Thaksen :

I agree with Mr.Hedge approach below, I believe Aramco as client will appove it considering there will only be slight difference between Client spec and ASME Requirement.

Just wondering, if this vessel to be U-stamped per ASME VIII, will AI sign the document if the minimum PWHT temp is not achi eved.

Please let me hear you thought guys..

Regards
Richard Bonardo
QA/QC Engineer
PHE-ONWJ



From: "hegde.pb@isgec.com" <hegde.pb@isgec.com>
To: materials-welding@googlegroups.com
Sent: Thu, 2 September, 2010 10:04:26 PM
Subject: Re: [MW:6834] tempering temperature of P4 material

In such case, it is better to approach client with all justification and docments and require to convince client , stating no deviation from code and spec.assuring to achieve all required test result
Also test the plate with revised simulation for impact value by which you can convince better
Regard
Hegde

Sent from my BlackBerry® smartphone from !DEA


From: THAKSEN INGOLE <t_ingole@yahoo.co.in>
Sender: materials-welding@googlegroups.com
Date: Thu, 2 Sep 2010 15:27:03 +0530 (IST)
To: material welding<materials-welding@googlegroups.com>
ReplyTo: materials-welding@googlegroups.com
Subject: [MW:6831] tempering temperature of P4 material


Dear all

There is a clause in Saudi Aramco documents stating as below

The maximum PWHT soaking temperature for quenched and tempered carbon steel and C-1/2Mo shall not exceed the temperature at which the test pieces were heat treated as shown on mill test reports or 650 deg C max for carbon steel ,690 deg C max for C-1/2 Mo and 700 for low Chrome alloy.

Our material is SA-387-Gr 12 cl2 (C -1/2Mo) which is P4 material. The min PWHT temp as per code (VIII Div 1-U stamp) is 650 deg C.

Now aramco has commented on our documents that they need a PWHT temperature to be 25 deg C less than tempering temperature as specified on MTC for the plates. So we need to have a tempering temp of min 680 deg C  so we can carry out the PWHT at 650 deg C but he plates MTC shows the tempering temp as 660 so we are 15-20 deg below. The plates are already purchased which are 65,70,80 mm thick.

My first query is no where in the aramco document we can find a clause of have PWHT temp 25 deg C less than tempering then what is the reason for asking this requirement.
What is the solution that we can offer them.

Regards
Thaksen  

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...