Skip to main content

Re: [MW:6825] Construction Code for Structural Steel (offshore construction)

Dear
 
NORSK M-101

This standard covers the requirements for fabrication and inspection of offshore steel structures with

SMYS < 500 MPa and with a minimum design temperature down to -14°C. For special application

steels with SMYS up to 690 MPa may be used.
 

6.10 Post weld heat treatment (PWHT)

PWHT shall be required for structural welds in steel quality level I or II, or quality level III with

Re>400MPa, when the nominal thickness (as defined in EN 288-3, section 8.3.2.1) exceeds 50 mm,

unless adequate fracture toughness can be documented in the as welded conditions. For restrained

joints of complicated design, PWHT may be required for smaller thicknesses, independent of steel

quality level.

PWHT shall be carried out in accordance with a procedure which shall include:

Heating rate.

Cooling rate.

Soaking temperature and time.

Heating facilities.

Insulation.

Control devices.

Recording equipment.

Configuration of structure to be PWHT or details if local PWHT shall be carried out.

Number and location of thermocouples to be used during PWHT.

The holding time and temperature shall be as recommended by the steel manufacturer


 
G.S.Arora
B4-103 LaHabitat
Opp Marutinandan Villa
Near Aayna Shopping Complex
Off SG Road Thaltej
AHMEDABAD-380054
Ph: 91-9725262404


--- On Wed, 1/9/10, sugu puma <pumamy@yahoo.com> wrote:

From: sugu puma <pumamy@yahoo.com>
Subject: Re: [MW:6820] Construction Code for Structural Steel (offshore construction)
To: materials-welding@googlegroups.com
Date: Wednesday, 1 September, 2010, 10:43 AM

Dear sir,
              Post weld heat treatment is compulsory requirement to offshore structures for relief stress concentration, try to review project requirements documents / design engineer,they are requirements from previous offshore structure crack happen in transocean/ensco semi.they normal plate rolling by making tubular for jacket platform
AWS D1.1 refer to post weld heat treatment code and material selection section ,

from,
M.sugu

From: omar fazni <ofazni@yahoo.com>
To: materials-welding@googlegroups.com
Sent: Wed, September 1, 2010 12:45:17 PM
Subject: [MW:6819] Construction Code for Structural Steel (offshore construction)

Dear All,
 
I would like to request information of any construction code that is applicable for offshore construction (structural steel), is there any code that determines PWHT requirements with regards of the material Thickness??.
 
For example, we're going to use a 2" tubular materials for offshore structural construction, is there any construction code saying that it has to be PWHT?? I've been looking in AWS D 1.1 and it stated that there are no requirements, except written in the contract
 
Please correct me if I'm wrong
 
Thank you & Regards
 
Ofazni

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...