Skip to main content

Re: [MW:6672] What is the Filler metal to weld Base metal (SA516 Gr 60) to achieve weld metal tensile properties after Normalization+ Stress Relieving

yes, it is acceptable, you can select higher metallurgy to get desired mech properties, as long as no restriction w.r.t corrosiveness of the fluid.

On Tue, Aug 24, 2010 at 10:55 AM, aly mhaskar <mhaskar_aly@yahoo.com> wrote:
Dear Mr. Karthik / Raghuram bathula
My Question is whether the filler metal
(SMAW with E9018-G; SFA 5.5; A=10; F no. 4 & SAW with F9P6 EG F3; SFA 5.23; A=10; F no. 6)
is acceptable to the base metal (SA516 Gr 60) as weld metal chemical properties(C=0.06%, Mn=1.37%, Si=0.24%, S% <0.005, P=0.014%, Mo=0.48%, Ni=0.82%, Cu=0.13%.) are not meeting the SA516 Gr60 requirements.
 
Aly
Kuwait



From: Karthik <karthik6684@yahoo.com>
To: materials-welding@googlegroups.com
Sent: Tue, August 24, 2010 7:32:00 AM
Subject: Re: [MW:6667] What is the Filler metal to weld Base metal (SA516 Gr 60) to achieve weld metal tensile properties after Normalization+ Stress Relieving

Hi,
I found the WPS&PQR from your Contractor have used SA516 Gr.&0(P.No.1,Gr.2) but your actual material in production is SA516 Gr.60(P.No.1,Gr.2). Change in Material Group No.is a Supplementary Essential Variable for SMAW and SAW Processes as per QW253 and QW254.
Please find below the extarction from ASME Section -IX-QW403.5 for your reference.
 

QW-403.5

Welding procedure specifications shall be

qualified using one of the following:

(a)

the same base metal (including type or grade) to be

used in production welding

(b)

for ferrous materials, a base metal listed in the same

P-Number Group Number in table QW/QB-422 as the base

metal to be used in production welding

(c)

for nonferrous materials, a base metal listed with

the same P-Number UNS Number in table QW/QB-422

as the base metal to be used in production welding

For ferrous materials in table QW/QB-422, a procedure

qualification shall be made for each P-Number Group Number

combination of base metals, even though procedure

qualification tests have been made for each of the two

base metals welded to itself. If, however, two or more

qualification records have the same essential and supplementary

essential variables, except that the base metals

are assigned to different Group Numbers within the same

P-Number, then the combination of base metals is also

qualified. In addition, when base metals of two different

P-Number Group Number combinations are qualified using

a single test coupon, that coupon qualifies the welding of

those two P-Number Group Numbers to themselves as well

as to each other using the variables qualified.

This variable does not apply when impact testing of

the heat-affected zone is not required by other Sections.


So,If impact testing is required in your case,your contractor shall do supporting PQR with the actual production material (SA516 Gr.60) otherwise the exising WPS and PQR of your contarctor is acceptable.
 
Thanks & Regards,
 
(karthik)



--- On Tue, 8/24/10, Aly <mhaskar.aly@gmail.com> wrote:

From: Aly <mhaskar.aly@gmail.com>
Subject: [MW:6663] What is the Filler metal to weld Base metal (SA516 Gr 60) to achieve weld metal tensile properties after Normalization+ Stress Relieving
To: materials-welding@googlegroups.com
Date: Tuesday, August 24, 2010, 1:51 AM

Dear All,
We are getting Heads for pressure vessels from Supplier in Saudi, The head requirements are as follows:
 
Head: 28mm thk; SA516 Gr 60, NACE MR 0175 & HIC tested NACE TM 0284
Construction Code ASME SEC VIII Div 1, E2007 Ad2009.
Type of Head Ellipsoidal with chordal seam (U stamped)
Service For Pressure vessel in Sour Service
HT: Normalization at 910deg C for  after forming & SR at 610 deg C along with vessel.
Chemistry restriction by Client: C= 0.06% Si=0.24%, S= 0.007 & P=0.015, Hardness 200BHN
Simulation Testing for HT (NR+SR) on test plate required.
 
 
Now the supplier has submitted me WPS / PQR for welding chordal seam of head for my review, the details of PQR as follows:
Base metal SA516 Gr70; 90mmthk
SMAW with E9018-G; SFA 5.5; A=10; F no. 4
SAW with F9P6 EG F3; SFA 5.23; A=10; F no. 6
HT= NR+SR
 
The weld metal composition achieved on PQR for SAW process are C=0.06%, Mn=1.37%, Si=0.24%, S% <0.005, P=0.014%, Mo=0.48%, Ni=0.82%, Cu=0.13%.
 
Tensile& bend test meeting requirements of Base metal.
 
My Question is whether the proposed filler metal is acceptable to this base metal (SA516 Gr 60) as per ASME SEC IX as weld metal chemical properties are not meeting the base metal requirements.
 
Thanks for co operation in this regard
 
Aly
Kuwait
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...