Pl. refer UCS 85
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Muhammed Ibrahim PK
Sent: Tuesday, August 17, 2010 9:16 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:6529] simulation treatment
Hi,
Simulation heat treatment is performing on sample piece of material to be used in production.
If the production required PWHT for 2 Hrs, do PWHT in the sample piece of the material for three cycle. ie 6hrs. then carry out the tensile test and hardness test & if applicable impact also.
If any production repair required we have to confirm the property of material is safe after multiple PWHT.
Thanks & Regards
Muhammed Ibrahim PK
On 16 August 2010 23:06, asad azmi <azmiasadayub@gmail.com> wrote:
Dear All,Greetings.what is simulation Treatment and where it is applicable.Please expalin with example in reference to ASME SEC VIII DIV 1/ASME SEC IIThanks in advance.RegardsAsad