[MW:6431] RE: 6399] MW: 6397- What type of Heat treatment to be done

Dear Sir

Following are the Inspection requirements from our client side:

 

(1) Electrode-ASME Sec II C SFA 5.9 ER 2594;

(2) The PQR shall be qualified as per ASME SEC IX & additional test as per API 938-C

(3) Tensile test, bend test, chemical test as per ASME SEC IX

(4) Ferric chloride corrosion test as per ASTM A 923 Method C

(5) Cross section macro examination; ferrite measurement & hardness testing.

(6) Heat input range to be specified in WPS.

(7) All weld location shall be checked for %  ferrite measurement.

 

 

Regards

Subrata Das

P. K. Tubes & Fittings Pvt. Ltd.

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pgoswami
Sent: Monday, August 09, 2010 5:01 PM
To: materials-welding@googlegroups.com
Subject: [MW:6399] MW: 6397- What type of Heat treatment to be done

 

What's the design code and applicable specifications(e.g NACE, API)....

 

Please provide these details.Duplex S.S can have different testing requirements based on the end services.

 

Thanks.

 

Pradip Goswami,P.Eng.

Welding & Metallurgical Engineer/Specialist

Ontario Power Generation Inc.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of subrata das
Sent: Monday, August 09, 2010 7:06 AM
To: materials-welding@googlegroups.com
Subject: [MW:6397] What type of Heat treatment to be done

Dear All

Can anyone suggest me which type of heat treatment to be carried out on a PQR test coupon.  My PQR test coupon is cladded plate Duplex SS UNS S32750 to SA516 Gr.70. Thickness of Duplex SS UNS S32750 is 3 mm and thickness of SA516 Gr.70 is 10 mm. This PQR to be used while welding in two part welded fittings.       

 

Regards

Subrata Das

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...