Skip to main content

RE: [MW:5984] RE: 0] RE: 0] RE: 5977] RE: 0] RE: 0] MW: 5945- Copper Base alloys

Hi Nilesh
You are absolutely right, we tried to convince our customer but he didn't agreed.
That's why we need to supply the coolers as per their requirements.
 
Thanks
Praphulla


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Darji Nilesh (Mumbai - Machinery)
Sent: Thursday, July 15, 2010 1:16 PM
To: 'materials-welding@googlegroups.com'
Subject: RE: [MW:0] RE: 0] RE: 0] RE: 5977] RE: 0] RE: 0] MW: 5945- Copper Base alloys

Your statement “customer requirement is very much stringent and also the outside atmosphere is salty & Corrosive”

 

If atm. Is salty/corrosive than that is applicable to complete Plant, You can use proper Painting cycles suitable for SALTY/Corrosive atm. But, I think, that is not the basic reason to change the basic material for Oil cooler Shell.

 

Nilesh Darji

 

CONFIDENTIALITY NOTICE

This e-mail and any attachments there to contain information, which is confidential, proprietary, privileged and/or protected from disclosure by intellectual property rights and are intended for the sole use of the recipient(s) named above. If you are not the intended recipient of this message you are hereby notified that any dissemination or copying of this message is strictly prohibited. If you have received this e-mail in error, please notify the sender either by telephone or by e-mail and delete it from any computer. Although this e-mail and any attachments thereto are believed to be free from any virus or other defects, which might affect any computer or IT system, it is the responsibility of the recipient to ensure that they are virus free. We are not liable for any loss or damage arising in any way from receipt or use there of. Thank you.

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Phirke, Praphulla D (GE Oil & Gas)
Sent: Thursday, July 15, 2010 10:45 AM
To: materials-welding@googlegroups.com
Subject: [MW:0] RE: 0] RE: 0] RE: 5977] RE: 0] RE: 0] MW: 5945- Copper Base alloys

 

Hi Ashok

I agree to your points but here customer requirement is very much stringent and also the outside atmosphere is salty & Corrosive so CS & SS options were out during the proposal stage itself.

Earlier customer has requested by Titanium Tube & Tubesheets with other parts as Monel.. But then suggested the other option of Cu NI tubes , AL Bronze tubesheets.

 

Thanks

Praphulla

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ashok Raman B Kutty (MNT/PPTSB)
Sent: Thursday, July 15, 2010 9:53 AM
To: materials-welding@googlegroups.com
Subject: [MW:0] RE: 0] RE: 5977] RE: 0] RE: 0] MW: 5945- Copper Base alloys

Lube oil coolers for compressors are small – approx 0.5m diameter and 3m long. You do not need to use non-ferrous materials for the shell since it will contain lube oil.

 

Typically, carbon steel is used for the shell (filters are in the lube oil circuit to remove any corrosion product), the tubesheets, baffles and tie-rods are made of non-ferrous materials, the tubes are integrally finned (SB 359).

 

If the customer does not want to use carbon steel for the shell, you could propose stainless steel which would be cheaper than a copper alloy.

 

If your first email had contained the info about the lube oil cooler, it would have kept everyone from guessing.

 

Ashok

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Praphulla Phirke
Sent: Thursday, July 15, 2010 12:53 AM
To: materials-welding@googlegroups.com
Subject: [MW:0] RE: 5977] RE: 0] RE: 0] MW: 5945- Copper Base alloys

 

Hi Ashok

Yes I am working on lube oil coolers for compressors .

 

Thanks

Praphulla

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ashok Raman B Kutty (MNT/PPTSB)
Sent: Wednesday, July 14, 2010 11:48 AM
To: materials-welding@googlegroups.com
Subject: [MW:5977] RE: 0] RE: 0] MW: 5945- Copper Base alloys

 

Praphulla,

 

Are you working on a lube oil cooler for a compressor?

 

Ashok

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Phirke, Praphulla D (GE Oil & Gas)
Sent: Wednesday, July 14, 2010 11:40 AM
To: materials-welding@googlegroups.com
Subject: [MW:0] RE: 0] MW: 5945- Copper Base alloys

 

Hi Pradip

Thanks a lot for your valuable input.

Answering to your query, there is no specific document issued by customer for material requirements, they have only suggested the materials for coolers as mentioned below during Kick of meeting

 

 

Design conditions are also normal like Design pressure is 10.2 Bar G & Design temperature is 90 Deg C. But here I have to provide the cooler with ASME U stamp

 

Do you foresee any issue with this?

 

Thanks

Praphulla


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pgoswami
Sent: Wednesday, July 14, 2010 7:12 AM
To: materials-welding@googlegroups.com
Subject: [MW:0] MW: 5945- Copper Base alloys


 

Hi  Praphulla,

 

I  looked at the requirements  and here is the summary:-

 

1.     Channel, Channel cover & Baffles  ASTM B 171 C61400--  Al-6.0-8.0, Fe-1.5-3.5, Balance  Cu.

 

2.    Tubes ASTM B-111 C71500— Cupro-Nickel- Ni-29.0-31.0, Fe -0.4-1.0, Balance Cu.

 

3.   Tube sheets ASTM B-171 C71500—As Above

 

4.    Pipes- seamless, copper alloy  in  nominal pipe sizes, both regular and extra strong--ASME ,SB-315, Alloy C61400

 

5.   Girth flanges, Nozzle flanges- Hot Forged SB 283 C 61900 (Max Fe content 4.0%, clause F of TABLE-1)  or SB-283 ,C-62300 or  ASTM B 124 C-61900 OR C-62300.

 

 

Note for 1,2,3 the identical ASME specification is available  as  in  Sec-II Part-B , SB 171 &  SB-111. Same applies for materials 4 & 5. Since the  exchanger design is as per ASME , Sec-VIII, DIV-1 , ASME spec ed  materials would be preferred over ASTM. 

 

What are the design conditions and specification requirements for materials. Does your client have any guidebook or specifications  for operating conditions vs materials requirements? 

 

 

Thanks

 

Pradip Goswami,P.Eng.

Welding & Metallurgical Engineer/Specialist

Ontario Power Generation Inc.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Phirke, Praphulla D (GE Oil & Gas)
Sent: Monday, July 12, 2010 2:38 AM
To: materials-welding@googlegroups.com
Subject: [MW:5945] RE: 5944] RE: 5943] RE: 5941] MW: 5927- Copper Base alloys

Hi Ashok

Process fluid is Shell side Oil VG 220 & Tube side Sea Water....

But customer specifically asked to follow these materials for both sides.

 

Thanks

Praphulla 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ashok Raman B Kutty (MNT/PPTSB)
Sent: Monday, July 12, 2010 12:02 PM
To: materials-welding@googlegroups.com
Subject: [MW:5944] RE: 5943] RE: 5941] MW: 5927- Copper Base alloys

Praphulla,

 

Some info, related to but not specific to your question ---

 

Sea water  is generally placed on the tube side of a floating head exchanger with HDPE inserts at the tube inlet ends to prevent erosion. In these cases, the tubes are made of non-ferrous material like aluminium brass, tubesheets of Al Ni bronze.

 

What is the process fluid?

 

 

Ashok

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Phirke, Praphulla D (GE Oil & Gas)
Sent: Monday, July 12, 2010 2:02 PM
To: materials-welding@googlegroups.com
Subject: [MW:5943] RE: 5941] MW: 5927- Copper Base alloys

 

Hi Pradip

Since I am dealing with these materials 1st time.. I need some more help from you.

Can you please suggest me the material of construction for the rest of the components of the heat exchanger?

 

Right now I am going ahead for Shell, Channel, Channel cover & Baffles as ASTM B 171 C61400 , Tubes ASTM B-111 C71500 , Tubesheets ASTM B-171 C71500

 

But for girth flanges, nozzle flanges which material is best one since its going to be welded to ASTM B 171 C61400? Can you please help me?

 

Thanks

Praphulla

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pgoswami
Sent: Monday, July 12, 2010 4:37 AM
To: materials-welding@googlegroups.com
Subject: [MW:5941] MW: 5927- Copper Base alloys

Praphulla,

 

General composition of  both the alloys are as follows.For sea water applications both the alloys are popular.Alloy C-63000(Ni-Al bronze) is an alloy with higher strength which could be attractive from design point of view and would be costlier than the other variety.

 

 

 

 

 

You may find the attached booklet as good information to start with.

Bronze alloys are  common cost effective choices in sea water applications, many times as castings. However if heat exchangers are to be fabricated entirely from this alloy, it would involve good fabrication practices.

Thanks.

Pradip Goswami,P.Eng.

Welding & Metallurgical Engineer/Specialist

Ontario Power Generation Inc.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Phirke, Praphulla D (GE Oil & Gas)
Sent: Saturday, July 10, 2010 3:13 AM
To: materials-welding@googlegroups.com
Subject: [MW:5927] Copper Base alloys
Importance: High

Dear all,

For one of my project, I have to use Sea water for cooling purpose.

For the same customer has suggested following materials for heat exchanger

 

Shell, Channel, Channel cover & Baffles as ASTM B 171 C61400 or ASTM B 171 C63000

 

I never used such type of materials earlier.

 

Can anyone suggest me which option is best option & why?

Also let me know which is costlier ?

 

Thanks

Praphulla

 

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

DISCLAIMER : This e-mail and any files transmitted with it ("Message") is intended only for the use of the recipient(s) named above and may contain confidential information. You are hereby notified that the taking of any action in reliance upon, or any review, retransmission, dissemination, distribution, printing or copying of this Message or any part thereof by anyone other than the intended recipient(s) is strictly prohibited. If you have received this Message in error, you should delete this Message immediately and advise the sender by return e-mail. Opinions, conclusions and other information in this Message that do not relate to the official business of PETRONAS or its Group of Companies shall be understood as neither given nor endorsed by PETRONAS or any of the companies within the Group.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

DISCLAIMER : This e-mail and any files transmitted with it ("Message") is intended only for the use of the recipient(s) named above and may contain confidential information. You are hereby notified that the taking of any action in reliance upon, or any review, retransmission, dissemination, distribution, printing or copying of this Message or any part thereof by anyone other than the intended recipient(s) is strictly prohibited. If you have received this Message in error, you should delete this Message immediately and advise the sender by return e-mail. Opinions, conclusions and other information in this Message that do not relate to the official business of PETRONAS or its Group of Companies shall be understood as neither given nor endorsed by PETRONAS or any of the companies within the Group.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

DISCLAIMER : This e-mail and any files transmitted with it ("Message") is intended only for the use of the recipient(s) named above and may contain confidential information. You are hereby notified that the taking of any action in reliance upon, or any review, retransmission, dissemination, distribution, printing or copying of this Message or any part thereof by anyone other than the intended recipient(s) is strictly prohibited. If you have received this Message in error, you should delete this Message immediately and advise the sender by return e-mail. Opinions, conclusions and other information in this Message that do not relate to the official business of PETRONAS or its Group of Companies shall be understood as neither given nor endorsed by PETRONAS or any of the companies within the Group.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...