RE: [MW:5893] PWHT Requirement of carbon steel (BS EN 10025 S275JR) plate 25mm to the plate (ASTM A387 Gr 11 Cl 2) 18mm THK

Assuming that the Grade 11 Class 2 plate (ASME Section IX, P4 material) is the pressure boundary material,  then PWHT is required per UCS-56. 

 

Requirements for exemption to PWHT requirement are covered in Note (2) to Table UCS-56 for P4 material.  PWHT can be forgone only for the following:

1.       Circumferential butt welds in pipe or tube with diameter less than 100mm, thickness less than 16mm, and carbon content  less than 0.15%

2.       Fillet welded non-pressure attachments to pipe or tube with diameter less than 100mm, thickness less than 16mm, and carbon content less than 0.15%

3.       Studs welded to pipe or tube with diameter less than 100mm, thickness less than 16mm, and carbon content less than 0.15%

4.       Electric resistance welded heat absorbing fins to pipe or tube with diameter less than 100mm and carbon content less than 0.15%

 

Clearly your description for fabrication does not meet any of the above four criteria.  Therefore PWHT is required.

 

John

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Dharmesh Mistry
Sent: Wednesday, July 07, 2010 6:57 AM
To: materials-welding@googlegroups.com
Subject: RE: [MW:5892] PWHT Requirement of carbon steel (BS EN 10025 S275JR) plate 25mm to the plate (ASTM A387 Gr 11 Cl 2) 18mm THK

 

Construction Code is Section VIII Division 1.

Weld Geometry: Groove + Fillet.

 

Best Regards,

 

Dharmesh Mistry

HEURTEY PETROCHEM

Tel. +91 22 67740074

Cell +91 98207 35814

Dharmesh.Mistry@heurtey.in

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Bathula Raghuram (Mumbai - PIPING)
Sent: Wednesday, July 07, 2010 5:10 PM
To: 'materials-welding@googlegroups.com'
Subject: RE: [MW:5891] PWHT Requirement of carbon steel (BS EN 10025 S275JR) plate 25mm to the plate (ASTM A387 Gr 11 Cl 2) 18mm THK

 

What is your construction code? , weld geometry is it butt or fillet?

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Dharmesh Mistry
Sent: Wednesday, July 07, 2010 4:57 PM
To: materials-welding@googlegroups.com
Subject: [MW:5889] PWHT Requirement of carbon steel (BS EN 10025 S275JR) plate 25mm to the plate (ASTM A387 Gr 11 Cl 2) 18mm THK

Dear all,

 

Is it required to do PWHT for fillet weld carbon steel (BS EN 10025 S275JR) plate 25mm to the plate (ASTM A387 Gr 11 Cl 2) 18mm THK?

 

Best Regards,

 

Dharmesh Mistry

HEURTEY PETROCHEM

Tel. +91 22 67740074

Cell +91 98207 35814

Dharmesh.Mistry@heurtey.in

 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...