[MW:5617] RE: 5606] Tube to tube sheet welding

The attached figure is from EN ISO 15614-8, "Specification and
qualification of welding procedure for welding materials - welding
procedure test - Part 8: Welding of tubes to tube-plate joints.
Minimum leak path dimension determination for ASME would be similar.

My company routinely manufactures ASME Section VIII heat exchangers and
fire tube boilers. What my company routinely does is to measure the
smallest distance from the root of the weld to the surface of weld as
part of the macro exam. Our acceptance criteria is that this measured
minimum distance must be greater than or equal to the wall thickness of
the tube. This is conservative but may preclude having to do push/pull
out testing. We have demonstrated for some customers that the tube will
fail outside of the weld when this criteria is adopted. Our J-groove is
always cut deeper than the tube wall thickness dimension.

Let me know if you have any additional questions.

John

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Shadab Alam
Ansari (Welding Engineer)
Sent: Tuesday, June 15, 2010 3:19 PM
To: Materials & Welding
Subject: [MW:5606] Tube to tube sheet welding

In Tube to tube sheet weld joint what is the minimum leak path
distance as per ASME SEC-IX.

Regards
Shadab Alam Ansari
Welding Engineer
Olayan Descon

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...