Skip to main content

RE: [MW:5089] Hydrotest of Piping System

Dear Puneet,

Please refer to ASME Sec. I, clause PG-99.1 states that "No part of the boiler shall be subjected to a general membrane stress greater than 90% of its yield strength at test temperature".

However, refer to ASME Sec. VIII Div. 2, Clause 4.1.6.2 specified that the hydrotest pressure shall not exceed 95% of yield strength for design basis. Also refer to Clause 8.2.1 of Div. 2, it specifies the minimum hydro test pressure which will be less than 95% yield stress of the material.

ASME B31.3, Clause 345.4.2 (c) specified that the hydrotest pressure is lesser of yield strength of the material.

ASME Sec. VIII Div. 1 does not indicate any limits on hydrotest. However, after hydro test "No visible permanent distortion" (UG-99(d)) shall be allowed.

Hence, most of the owners/ designers/ manufacturer will limit the hydrotest level to 90% of SMYS in order to protect from permanent distortion for particular piping system/ vessels etc.

Regards,

L. Prabhu kumar,
Sr. Principal Engineer,

Equipments & Materials Dept.,
Saipem India Projects Limited,
Nungambakkam High Road, Chennai - 600 034, India.
Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,
Mobile Ph. No.: +91 9003010978.

-----Original Message-----
From: puneet takiar [mailto:puneet1takiar@yahoo.com]
Sent: Wednesday, May 05, 2010 7:29 PM
To: Prabhu Kumar L
Subject: Re: [MW:5073] Hydrotest of Piping System

Dear sir,
whether these factor of safeties are mentioned in some standard or tables?

Regards,
puneet takiar
________________________________

----- Original Message ----
From: Prabhu Kumar L <l.prabhukumar@saipem-india.com>
To: materials-welding@googlegroups.com
Sent: Tue, 4 May, 2010 4:27:02 PM
Subject: RE: [MW:5073] Hydrotest of Piping System

Dear All,

Further to the trailing mail, I would like to add some more points. The
basic criteria for any hydrotest (piping, equipment or pipeline) is that
the hydro test pressure shall not exceed 0.9 times of yield strength of
the materials which is being hydro tested.

The maximum hydro test pressure is arrived based on factor of safety
multiplied by the times of design pressure. For ex. All onplot piping,
the factor of safety is 0.6 and hydro test pressure is 1.5 times of
design pressure. Hence, 0.6 x 1.5 = 0.9, same way for pipeline, the
factor of safety is 0.72 and hydrotest pressure is 1.25 times of design
pressure, which comes 0.9. (the times of design pressure may vary
depends on factor of safety)

It means that at any point of time the hydrotest pressure shall not
exceed 90% of yield strength of the material and also it is decided
based on design factor or factor of saftey. If it exceeds this limit,
the material shall undergo permanent/ plastic deformation and this shall
not be rectified. Hence as long as the hydro test pressure is within
this limit, the system will work (immaterial of number of times).

Regards,

L. Prabhu kumar,
Sr. Principal Engineer,

Equipments & Materials Dept.,
Saipem India Projects Limited,
Nungambakkam High Road, Chennai - 600 034, India.
Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,
Mobile Ph. No.: +91 9003010978.

L. Prabhu kumar,
Sr. Principal Engineer,

Equipments & Materials Dept.,
Saipem India Projects Limited,
Nungambakkam High Road, Chennai - 600 034, India.
Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,
Mobile Ph. No.: +91 9003010978.

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Darcy Morin
Sent: Tuesday, May 04, 2010 7:49 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:5064] Hydrotest of Piping System

Further, ASME B31.3 utilizes a 3:1 safety factor in the Allowable 
Stress Design of piping systems. So, it is unlikely that a 150% 
hydrotest will weaken the system.

On 2010-05-04, at 0:37, Kathalingam Babu <kathalingam.qaqc@ppl.com.sg
wrote:

> Hi
>
> On top of below mail, the materials will be weaken only if the test 
> pressure exceeds the yield strength of the materials.
>
> In all codes, the test pressure will consider the above fact and 
> test temperature, so the weakening of materials is rare if you 
> follow appropriate fabrication procedures.
>
> Consideration shall be given what was the cause of failure, rather 
> than how many time hydrotest allowed.
>
> Rgds,
>
> K.Babu
>
>
> ----- Original Message ----- From: "Kathalingam Babu"
<kathalingam.qaqc@ppl.com.sg
> >
> To: <materials-welding@googlegroups.com>
> Sent: Tuesday, May 04, 2010 2:22 PM
> Subject: Re: [MW:5042] Hydrotest of Piping System
>
>
>> Hi
>>
>> For your info, if the system fails , it doesn't mean, your weaking 
>> the materials.
>>
>> I don't think , there is any restriction on how many times the 
>> hydrotest allowed.
>>
>> Rgds,
>>
>> K.Babu
>> Singapore
>>
>>
>> ----- Original Message ----- From: "dhinesh gnanadhas"
<dhineshlhmm@gmail.com
>> >
>> To: "Materials & Welding" <materials-welding@googlegroups.com>
>> Sent: Tuesday, May 04, 2010 2:03 PM
>> Subject: [MW:5042] Hydrotest of Piping System
>>
>>
>>> Hi.
>>>
>>> If the piping system getting fails in every test. Howmany times we 
>>> can
>>> do the hydro test for the same piping system?
>>>
>>> If we are doing the the hydrotest, we are weakening the pipe 
>>> material.
>>> So, Howmany times the same system can be allowed to retest?
>>>
>>> --
>>> To post to this group, send email to
materials-welding@googlegroups.com
>>> To unsubscribe from this group, send email to
materials-welding-unsubscribe@googlegroups.com
>>> For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
>>> The views expressed/exchnaged in this group are members personel 
>>> views and meant for educational purposes only, Users must take 
>>> their own decisions w.r.t. applicable code/standard/contract 
>>> documents.
>>>
>
>
> --
> To post to this group, send email to materials-
> welding@googlegroups.com
> To unsubscribe from this group, send email to
materials-welding-unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel 
> views and meant for educational purposes only, Users must take their 
> own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.


-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or

entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged

information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution

or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If

you have received this communication in error, please notify us immediately by responding to this email and then

delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete

transmission of the information contained in this communication nor for any delay in its receipt.
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or

entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged

information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution

or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If

you have received this communication in error, please notify us immediately by responding to this email and then

delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete

transmission of the information contained in this communication nor for any delay in its receipt.
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...