Re: [MW:5074] Pre Qualified Fillet Weld WPS as per AWS D1.1

Hi Sahul,
 
3G vertical Up qualifies all position including fillet welds provided the design or Spec. shall call for the CVN requirements.
 
Otherwise this variable doesn't valid,  In this case 3G qualifies 3F position only.
 
"Note 4" of Table 4.2,  you can apply very well on the Prequalified WPS as well.
 
Rgds,
 
K.Babu
 
 
----- Original Message -----
From: Shahul
Sent: Wednesday, May 05, 2010 2:40 AM
Subject: Re: [MW:5069] Pre Qualified Fillet Weld WPS as per AWS D1.1

Dear Devarajan,

Thanks for your quick reply..
As per my understanding, AWS D1.1 Table 4.2, is a table for "qualified" WPS. So i am confused whether, i can apply "note 4" in prequalified WPS. please clarify.

And also, as per Table 4.1, it clearly shows that, for a WPS qualified in 3G position, can only be used in "V" , ie 3F position. Then how can you say that, 3G complete penetration single groove welding WPS is sufficient for welding 1F and 2F ???


Regards,

Shahul

On Tue, May 4, 2010 at 5:15 AM, Devarajan Ramasamy <neo.devarajan@gmail.com> wrote:
I would like to add on to my comment.

Since your requirement for fillet is only 1F and 2F (namely flat and Horizontal), your 3G complete penetration single groove welding WPS is sufficient provided that the thickness and diameter matches.


On Tue, May 4, 2010 at 10:09 AM, Devarajan Ramasamy <neo.devarajan@gmail.com> wrote:

According to AWS D1.1 Section, Table 4.2  Note 4 clearly states that 


"CJP Groove weld qualifications on any thickness or diameter shall qualify any size of fillet or PJP Groove Weld for any thickness or diameter."


So, you can use your prequalified WPS on Single V Groove Complete Joint Penetration for fillet weld qualifications as long as the thickness and diameter matches.

Table 4.1 clearly shows the position qualified for each weld type and position in WPS.

I would suggest that you make your qualifications either in 2G, 3G and 4G if your qualification test piece is plate or a 6G if your qualification test piece is pipe as the range calls for.

Hope this helps.





On Mon, May 3, 2010 at 8:56 PM, Shahul <shahulhrj@gmail.com> wrote:


Dear All,

We have qualified a single V groove welding procedure in 3G position as per AWS D1.1. With this procedure, i can only do 3G in groove and 3F in Fillet. So i have prepared pre qualified single V groove WPS for groove welding in all positions.

But we have some jobs which demand 1F and 2F positions. So, i want to know whether prequalified WPS for the single V which i made is acceptable for doing fillet welding in all positions?? Or is there any prequalified WPS for fillet available ??

--
Thanks and Regards

Shahul

QC WELDING ENGINEER
CSWIP 3.1, AWS CWI
Aasia Steel Factory Co. Ltd
KSA


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
This message originated from the Internet. Its originator may or may not be who they claim to be and the information contained in the message and any attachments may or may not be accurate.

This email transmission is intended solely for the named recipient(s). It may contain confidential and/or privileged information.If you are not the intended recipient, note that disclosing, copying or distributing it may be unlawful. Please notify the sender immediately if you have received it by mistake, and delete it from your system.
Internet communications cannot be guaranteed to be timely, secure, error or virus-free. The sender does not accept liability for any errors or omissions.

"SAVE PAPER - THINK BEFORE YOU PRINT!"

Regards,

~ DEVARAJAN RAMASAMY~



--
This message originated from the Internet. Its originator may or may not be who they claim to be and the information contained in the message and any attachments may or may not be accurate.

This email transmission is intended solely for the named recipient(s). It may contain confidential and/or privileged information.If you are not the intended recipient, note that disclosing, copying or distributing it may be unlawful. Please notify the sender immediately if you have received it by mistake, and delete it from your system.
Internet communications cannot be guaranteed to be timely, secure, error or virus-free. The sender does not accept liability for any errors or omissions.

"SAVE PAPER - THINK BEFORE YOU PRINT!"

Regards,

~ DEVARAJAN RAMASAMY~

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...