Skip to main content

Re: [MW:5030] RE: 4998] mode of metal transfer in mig welding

depends on current and voltage setting, gas shielding. voltage if less than 22 volt will be in short circuit mode only even if u use mixture of argon + co2
kgp

On Thu, Apr 29, 2010 at 9:19 AM, John Henning <jhenning@deltak.com> wrote:
AWS welding handbook says the following for CO2 with GMAW:
 
. . . "With a CO2 shield, the metal transfer mode is either short circuiting or globular.  Axial spray transfer requires an argon shield and cannot be achieved with a CO2 shield.  With globular transfer the arc is quite harsh and produces a high level of spatter."  (implied if transfer is globulr then) "This requires that CO2 welding conditions be set to provide a very short "buried arc" (the tip of the electrode is actually below th surface of the work in ordre to minimize spatter."
 
In the US, when CO2 is used as a shielding gas, the transfer mode is nearly always short circuiting arc transfer (dip).  My understanding is that in Europe globular transfer is not uncommon, but I have little experience with it in actual welding.  If your process is short circuiting transfer, and ASME Sc IX is to be applied you will need to take into account essential variables QW-403.10 and QW-404.32 which may limit the qualified thickness of base metal and filler metal.  For QW-409.2 you willhave to list the transfer mode as short circuiting (dip).
 
Hope this helps.
 
John


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of durga bala suresh
Sent: Thursday, April 29, 2010 10:43 AM
To: materials-welding@googlegroups.com
Subject: [MW:4998] mode of metal transfer in mig welding

Dear Members,
we are going to qualify MIG welding process.
How to differentiate metal transfer like dip, globular & spray?
we are using IS 2062 material with 99.9% CO2 shielding gas,1.2 dia filler wire,12mm thick in single '' V'' Grove  butt Joint.
what is the desired testing requirements ? depending of metal transfer as per section IX 

thanks and regards,
Suresh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...