Dear NAUTIYAL,
 
since the MOC is SS304L with 8m dia, 30 mm thick having  3 long seam within one shell course following should be the approach of welding for better control on distoration.
 
1) weld preparation equal V .
2) Setup of seam in vertical axis with fixturing.
3) use of DOT with GTAW.
4) then parallel welding with SMAW from both side.
 
After welding with DOT SMAW ned to be comenced in free condition from both side for better control
 
SAW should be avoided in such type of joints
 
Amarjit Singh 
TEMA INDIA LTD
 


 
On Thu, Apr 8, 2010 at 12:20 AM, PREM SHANKARDUTT NAUTIYAL <prem_nautiyal@rediffmail.com> wrote:
Hi friends

The Job is a vessel and construction code is ASME Sec III NB.
The MOC is SS304L.
The O.D of the shell is 8 (eight) metres, thickness = 30mm, Height of shell is 2700mm.
We want to fabricate two shells of this type.
Each shell has three long seams.
Then both these two shells will be welded by one circ. seam.
I have decided a double V joint with SMAW process from inside welding.
From inside of the shell there will be lot of spiders / fixturing.

I have a few queries:

1)can i deploy SAW process from outside after chipback ?
2) What dia. of SAW wire i have to use ?
3)Can SAW boom reach at such height of 8 metres ?
We have a Lincoln SAW power source of 1200 A.

4)Has anyone used SAW for SS welding of such huge diameters in past ??

5)What is the optimum thickness in SS that can be welded by SAW to get least distortion ?

The PQR calls for ASME SecIX tests + IGC practice E requirements to be met..
6)Can we use Double operator TIG and then SMAW from Inside + SAW from outside ?

Regards

Prem Nautiyal

PREM S NAUTIYAL
CELL : 9820313278

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Amarjit Singh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...