Skip to main content

RE: [MW:4801] PWHT of Hydrotesting vents in Sour gas service

Dear Suresh,

 

If you want avoid PWHT, you can carryout mock-up test weld to test hardness within HRC 22 and can be proposed to client for approval. E7018 or ER70S-2 type filler metal can be used. Since, it is only for seal welding, client may accept the proposal.

 

L. Prabhu kumar,

Sr. Principal Engineer,

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of suresh venkat
Sent: Monday, April 12, 2010 5:57 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:4800] PWHT of Hydrotesting vents in Sour gas service

 

 

Hi,

 

Material of nconstruction is Carbon steel suitable for sour gas service with P & S restriction. Code- B31.3.

 

In original plan, all Sour gas pressure pipeline Hydrotest vents were of flanged connection with Blind flange.

 

in the exisiting plant, we encountered lot of leakages in this flanged joint which leads to emergency shutdowns.

 

So we want to avoid flanged joints for closing Hydrotest vents. The no. of hydrotest vents are more, there is a serious concern

 

Our specification says threaded joints are not acceptable for Sour gas service, as there is possiblity of leakge due to corrosion.

 

To balance all the criterias, we planned to provide threadolet on the pipelines as hydrotest vent.

 

After PWHT & hydrotest all the vent ends will be closed with Plugs( threaded joint).

 

 To avoid any leakage we want to provide a seal weld (fillet joint). as the rating of joints are 600# & above.

 

This fillet joint is critical as we don't want to end up again in same trouble in a different way.

 

 

Please advise on avoiding PWHT for this joint & suitable electrode for this CS joint.

 

Thanks 

 

Suresh 

 

 

 

 

 

 

 

 

 



 

On Mon, Apr 12, 2010 at 2:40 PM, Kathalingam Babu <kathalingam.qaqc@ppl.com.sg> wrote:

Hi

 

May i know, which spec. says , sour gas service needs mandatory PWHT ?

 

Regards,

 

K.Babu

 

----- Original Message -----

Sent: Monday, April 12, 2010 12:30 PM

Subject: RE: [MW:4793] PWHT of Hydrotesting vents in Sour gas service

 

Dear Suresh,

 

Please note that the intension of PWHT is to relieve the stresses from HAZ and weld metal as well. Use of Inconel or any other electrodes will not relieve the stresses from HAZ, and it remains same for all electrodes. Hence you cannot avoid PWHT. In order to reduce difficulties in PWHT you can propose the method as follows.

 

  • Buttering (weld overlay) of 5mm (if it is CS you can use same electrode) on the locations where weldolets to be welded to main pipeline.
  • After buttering, local PWHT shall be carried out as per procedure.
  • Welding between weldolet to buttered layer shall be done without PWHT.

 

The HAZ is a critical area which need to stress relieved. Also note that in general, the weld metal is softer than HAZ since, it contains very low % carbon and other minor alloying elements to improve slight toughness also.

 

Regards,

 

L. Prabhu kumar,

Sr. Principal Engineer,

 

Equipments & Materials Dept.,

Saipem India Projects Limited,

Nungambakkam High Road, Chennai - 600 034, India.

Tel:+91 44 43906588, Ext.: 588, Fax:+91 44 66840345,

Mobile Ph. No.: +91 9003010978.


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of suresh venkat
Sent: Sunday, April 11, 2010 4:49 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:4786] PWHT of Hydrotesting vents in Sour gas service

 

My intention was to weld with Inconel Electrode  so as to have soft weld metal.

 

Further opinions will be more helpful.

On Sun, Apr 11, 2010 at 4:10 PM, Raghuram Bathula <raghurambathula@gmail.com> wrote:

what if you weld with SS (ER/E309) or Inconel? members pl share ur opinion

 

On Sat, Apr 10, 2010 at 10:46 PM, suresh <atozsuresh@gmail.com> wrote:

we have sour gas pipelines with higher & lower pressure. All the
pipelines are with Hydrotest vents which will be closed after
Hydrotest.

For low pressure pipelines we use flanged joint with a Blind flange.
For high pressure pipe line with flanged connection there is
intermittent leakages which needs immediate attention even sometimes a
shut down.

We  intend to use a threadolet as vent & will be plugged & seal welded
after hydrotest. The problem is with PWHT. As all the lines in Sour
gas services shall be PWHT.

We want to avoid PWHT of this small fillet joint, Due to the location
of these joints & difficulty in PWHT. but it is dangerous to leave it
without PWHT as it may crack due to residual stresses.

Can you suggest any welding procedure & electrode to have this welding
with reduce hardness HRC 22 Max  by which PWHT can be avoided.

Thanks

Suresh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

To unsubscribe, reply using "remove me" as the subject.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

 

 


-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or 
entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged 
information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution 
or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If 
you have received this communication in error, please notify us immediately by responding to this email and then 
delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete 
transmission of the information contained in this communication nor for any delay in its receipt. 
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--

To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

 




-------------------------------------------------------------------------------------------------------------------------------------------------------------------
DISCLAIMER: The information contained in this communication is intended solely for the use of the individual or 
entity to whom it is addressed and others authorized to receive it. It may contain confidential or legally privileged 
information. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution 
or taking any action in reliance on the contents of this information is strictly prohibited and may be unlawful. If 
you have received this communication in error, please notify us immediately by responding to this email and then 
delete it from your system. Saipem India Projects Limited (SIPL) is neither liable for the proper and complete 
transmission of the information contained in this communication nor for any delay in its receipt. 
-------------------------------------------------------------------------------------------------------------------------------------------------------------------

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...