Senthil,
Yes it is permitted by QW 200.4.
But before proceeding SAW process on GTAW process, You have to see the nature of Joint , otheriwse it may lead to 'Burn Through'.
There is one more option provided you have time, you take one more test coupon and weld it with fCAW process and use this process as buffer layer.
I hopeit will help you.
Regards
rl garg
On Sat, 06 Mar 2010 18:31:55 +0530 wrote
>Dear Senthil,
As suggested by other members, its not an issue to make another WPS using only two proceses (with their qualified thicknes).
In my experience welding direct SAW on GTAW root may produce burn through. I hope that you have suffecient thickness for GTAW. Minimum thickness for GTAW shall be approx 8-10mm to weld directly SAW on it.
If possible try to weld mock up to confirm the feasibility before you prepare a new WPS using existing PQR.
Regards.
CK.
On 5 March 2010 07:54, SENTHILKUMAR SWAMINATHAN wrote:
Dear All,
I have qualify the PQR using proposed wps Process are GTAW/SMAW/SAW.
After all NDT & DT completed on same and actual WPS prepared and production weld also done using that WPS with same welding process.
Now my production dept want to rewrite the WPS using only GTAW & SAW due to repairs on production welds. Because repairs are @ SMAW weld location.
QW-200.4 is permitting this?
Thank you,
Regards,
S.Senthilkumar
The INTERNET now has a personality. YOURS! See your Yahoo! Homepage.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
C. K. Purohit
Eng-Tech Weld1
Sr Welding Inspector
--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Yes it is permitted by QW 200.4.
But before proceeding SAW process on GTAW process, You have to see the nature of Joint , otheriwse it may lead to 'Burn Through'.
There is one more option provided you have time, you take one more test coupon and weld it with fCAW process and use this process as buffer layer.
I hopeit will help you.
Regards
rl garg
On Sat, 06 Mar 2010 18:31:55 +0530 wrote
>Dear Senthil,
As suggested by other members, its not an issue to make another WPS using only two proceses (with their qualified thicknes).
In my experience welding direct SAW on GTAW root may produce burn through. I hope that you have suffecient thickness for GTAW. Minimum thickness for GTAW shall be approx 8-10mm to weld directly SAW on it.
If possible try to weld mock up to confirm the feasibility before you prepare a new WPS using existing PQR.
Regards.
CK.
On 5 March 2010 07:54, SENTHILKUMAR SWAMINATHAN
Dear All,
I have qualify the PQR using proposed wps Process are GTAW/SMAW/SAW.
After all NDT & DT completed on same and actual WPS prepared and production weld also done using that WPS with same welding process.
Now my production dept want to rewrite the WPS using only GTAW & SAW due to repairs on production welds. Because repairs are @ SMAW weld location.
QW-200.4 is permitting this?
Thank you,
Regards,
S.Senthilkumar
The INTERNET now has a personality. YOURS! See your Yahoo! Homepage.
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
--
C. K. Purohit
Eng-Tech Weld1
Sr Welding Inspector
--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments